A wear-resistant and puncture-resistant BOPP cosmetic film and preparation method thereof
By adding ultra-high viscosity silicone, anti-adhesive masterbatch, antistatic masterbatch and nano-titanium dioxide grafted hyperbranched polymer composite to the BOPP cosmetic film, the problem of insufficient wear resistance and puncture resistance of the BOPP film is solved and achieved It has similar performance improvements to POF film, improving the durability and use experience of cosmetic packaging.
Patent Information
- Application Number
- CN202310124576.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-16
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-02-16
AI Technical Summary
In the application of BOPP film in the field of cosmetics, its wear resistance and puncture resistance are insufficient, resulting in surface friction and scratches during transportation or handling, giving people a poor experience and limiting its application.
The BOPP cosmetic film adopts a three-layer structure, including an upper surface layer, a core layer and a lower surface layer. By adding ultra-high viscosity silicone, anti-stick masterbatch, antistatic masterbatch and nano-titanium dioxide grafted hyperbranched polymer composite materials, the film is improved Improved friction coefficient, anti-adhesion, electrostatic properties and wear resistance, reducing heat sealing temperature.
It has significantly improved the wear resistance and puncture resistance of BOPP film, achieving the same or even better results than POF film, improved transparency and heat sealing performance, and enhanced user experience.
Smart Images

Figure GDA0004991363170000061 
Figure GDA0004991363170000071
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of BOPP films, and in particular to a wear-resistant and puncture-resistant BOPP cosmetic film and a preparation method thereof. Background Art
[0002] Polyolefin heat shrink film, or POF film, is commonly used in cosmetic packaging. POF film has advantages in wear resistance and puncture resistance, but it also has problems such as general transparency and ugly hot seal. If BOPP film is used for packaging, the packaging grade will be greatly improved. First, with BOPP film, the transparency can be less than 1%, and the pattern or LOGO of the packaging box can be clearly seen; secondly, the packaging interface adopts overlapping heat sealing, like cigarettes and playing cards, and the seal is relatively flat, which greatly changes the zipper wrinkles and pricking experience of POF seal; thirdly, once BOPP film is used, the gold pull line can be used, which is very convenient when opening, while POF must be torn open with great force or using auxiliary tools such as scissors, and the gold pull line gives consumers a very good consumer experience.
[0003] In view of the above three advantages, there is a good prospect for using BOPP film to replace cosmetic film. However, in actual application, the wear resistance and puncture resistance of BOPP film are insufficient. During transportation or handling, its surface is scratched by friction, which gives people a poor experience and limits the application of BOPP film in the cosmetic field. Summary of the invention
[0004] In order to improve the wear resistance and puncture resistance of BOPP cosmetic films, the present application provides a wear-resistant and puncture-resistant BOPP cosmetic film and a preparation method thereof.
[0005] In a first aspect, the present application provides a wear-resistant and puncture-resistant BOPP cosmetic film, which adopts the following technical scheme: a wear-resistant and puncture-resistant BOPP cosmetic film, wherein the BOPP cosmetic film is made of a three-layer structure of an upper surface layer, a core layer and a lower surface layer through co-extrusion and compounding;
[0006] The upper surface layer comprises the following raw materials in parts by weight: 59-78 parts by weight of copolymerized polypropylene, 10-15 parts by weight of slip masterbatch, 2-6 parts by weight of anti-sticking masterbatch, and 10-20 parts by weight of elastomer; the slip masterbatch is prepared by mixing ultra-high viscosity silicone and copolymerized polypropylene in a weight ratio of 1:(8-10);
[0007] The core layer comprises the following raw materials in parts by weight: 96-98 parts by weight of homopolypropylene and 2-4 parts by weight of antistatic masterbatch;
[0008] The lower surface layer comprises the following raw materials in parts by weight: 70-80 parts by weight of copolymerized polypropylene and 20-30 parts by weight of elastomer.
[0009] By adopting the above technical scheme, the purpose of adding a slippery masterbatch to the upper surface of the film is to obtain a lower friction coefficient, so that the upper surface of the film can run more smoothly when in contact with the metal surface of the packaging equipment; the purpose of adding an anti-sticking masterbatch is to prevent the film from becoming sticky during production or use and to improve the opening property; the purpose of adding an antistatic masterbatch to the core layer of the film is to effectively reduce the impact of static electricity on packaging during production, transportation, and machine operation; the purpose of adding an elastomer to the upper and lower surface layers of the film is to reduce the heat sealing temperature to meet the customer's requirements for low-temperature heat sealing and puncture resistance, and it also has a positive additive effect on improving wear resistance; the slippery masterbatch abandons the common silicone oil in the industry, which can further improve the wear resistance of the film surface. Through the mutual synergy between the raw materials, the original wear resistance is taken to a higher level, completely achieving the same effect as POF, or even better.
[0010] Preferably, the ultra-high viscosity silicone has a viscosity of 500,000-1,000,000 at 25°C.
[0011] By adopting the above technical solution, the viscosity of the ultra-high viscosity silicone can be within this range.
[0012] Preferably, the upper surface layer further comprises 1-5 parts by weight of a nano-titanium dioxide grafted hyperbranched polymer composite material.
[0013] By adopting the above technical scheme, by adding nano-titanium dioxide grafted hyperbranched polymer composite materials, the film hardness of BOPP cosmetic film can be improved, the nano-titanium dioxide grafted hyperbranched polymer composite materials can cooperate with the silicon dioxide in the system, and the nano-titanium dioxide grafted hyperbranched polymer composite materials can fill the interface pores between silicon dioxide and the system, thereby improving the wear resistance of the film.
[0014] As a preferred method: the preparation method of the nano-titanium dioxide grafted hyperbranched polymer composite material is as follows:
[0015] 1) Add 4.5-5.5 parts by weight of nano titanium dioxide to 30-35 parts by weight of xylene, disperse by ultrasonication, then add 4-6 parts by weight of water, 2-4 parts by weight of ethanol and 80-90 g of vinyltrimethoxysilane, adjust the pH of the system to 5-6, stir and react at 50-60° C. for 7-9 hours to obtain silane coupling agent modified nano titanium dioxide;
[0016] 2) adding 1-2 parts by weight of hydrolyzed polymaleic anhydride, 5-7 parts by weight of 2-aminoterephthalic acid, 2-3 parts by weight of diisopropanolamine, 2-3 parts by weight of triethanolamine and 0.25-0.35 parts by weight of n-propyl titanate to 5-6 parts by weight of DMF, heating to 125-135° C., stirring and reacting for 20-24 hours to obtain a hyperbranched polymer;
[0017] 3) Under a nitrogen atmosphere, add 3-4 parts by weight of silane coupling agent-modified nano-titanium dioxide to 6-8 parts by weight of DMF, then add 4-6 parts by weight of vinyltrimethoxysilane and 1-2 parts by weight of the hyperbranched polymer prepared in step 2), stir for 1-2 hours, add 0.003-0.005 parts by weight of initiator, stir at 70-80° C. for 20-24 hours, filter, and dry to obtain a nano-titanium dioxide grafted hyperbranched polymer composite material.
[0018] By adopting the above technical scheme, by grafting a silane coupling agent on the surface of nano-titanium dioxide and then reacting with a hyperbranched polymer, the silane coupling agent structure and the hyperbranched structure grafted on the surface of the nano-titanium dioxide can be obtained. The silane coupling agent can reduce the interface energy between the nano-titanium dioxide and the system, making it difficult to leave pores between the nano-titanium dioxide and the system, thereby reducing the wear resistance of the film. In addition, the hyperbranched structure can reduce the viscosity of the nano-titanium dioxide grafted hyperbranched polymer composite material, making it more dispersible.
[0019] Preferably, the average molecular weight of the hydrolyzed polymaleic anhydride is 400.
[0020] By adopting the above technical solution, the average molecular weight of the hydrolyzed polymaleic anhydride should not be too large, otherwise it will easily reduce the dispersibility of the nano-titanium dioxide grafted hyperbranched polymer composite material.
[0021] Preferably, the elastomer used in the upper surface layer and the lower surface layer is a copolymer of propylene and butene, and the butene added during the preparation of the elastomer accounts for 5-10wt% of the total weight of propylene and butene.
[0022] By adopting the above technical solution, adding elastomers to the upper and lower surface layers of the film can reduce the heat sealing temperature, meet the customer's requirements for low-temperature heat sealing and puncture resistance, and also have a positive additive effect on improving wear resistance; a small amount of elastomer is added to the upper and lower surface layers, the main components of the elastomer are C3 and C4, of which C3 accounts for 90-95wt%, and the refractive index is very close to that of BOPP material, so it has high transparency. The Vicat softening point of the elastomer is 75°C, while the Vicat softening point of the surface copolymer polypropylene is 105°C. With such a large gap, only a small amount of addition is needed to reduce the heat sealing temperature again. Because of the addition of the elastomer, the flexibility of the film is further improved. With the joint addition of the low-temperature heat sealing material and the elastomer, the puncture resistance requirement of the cosmetic film is well solved.
[0023] Preferably, the antistatic masterbatch is made of homopolypropylene and nonionic glyceryl monostearate, and the mass percentage concentration of nonionic glyceryl monostearate in the antistatic masterbatch is 15%.
[0024] By adopting the above technical solution, antistatic masterbatch is added to the core layer of the film in order to effectively reduce the impact of static electricity on packaging during production, transportation, machine operation, etc.
[0025] Preferably, the upper surface anti-sticking masterbatch is made of copolymerized polypropylene and silicon dioxide, the mass percentage concentration of silicon dioxide in the anti-sticking masterbatch is 4.5-5.5%, and the particle size of silicon dioxide is 4 μm.
[0026] Preferably, the thickness of the BOPP cosmetic film is 28 μm, the thickness of the upper surface layer is 1-1.5 μm, the thickness of the core layer is 25-26 μm, and the thickness of the lower surface layer is 1-1.5 μm.
[0027] By adopting the above technical solution, by setting the thickness of the BOPP cosmetic film, the thickness of its upper surface layer does not need to be too high, so as to achieve excellent wear resistance; and the thickness of this product is relatively thin, which meets the requirements of lightweight product.
[0028] In a second aspect, the present application provides a method for preparing a wear-resistant and puncture-resistant BOPP cosmetic film, which adopts the following technical scheme:
[0029] A method for preparing a wear-resistant and puncture-resistant BOPP cosmetic film, comprising the following preparation steps:
[0030] 1) After the raw materials of the core layer are uniformly mixed and dried, they enter a melting single screw extruder and a metering single screw extruder connected in series for melting and plasticization, and then pass through a coarse filter, a metering pump, and a main filter to enter a die head. The temperature of each section is set to 220-250° C., and the melt temperature is 210-270° C.;
[0031] 2) The raw materials of the upper surface layer and the lower surface layer are mixed uniformly and dried, and then enter respective single-screw extruders for melt plasticization, and then pass through filters and metering pumps and enter die heads. The temperature of each section is set to 220-240° C., and the melt temperature is 220-250° C.;
[0032] 3) The three layers of polymer melt flow out after converging at the die head, and under the action of the air knife attachment device, adhere to the surface of the quench roller, and form a solid casting sheet after rapid cooling by the quench roller and the water tank, and then undergo longitudinal and transverse stretching in sequence; the longitudinal preheating temperature is 95-125°C, the stretching temperature is 70-100°C, the setting temperature is 80-130°C, and the longitudinal stretching ratio is 5.0-7.5; the transverse preheating temperature is 170-200°C, the stretching temperature is 130-160°C, the transverse stretching ratio is 8-10, the setting temperature is 155-175°C, and the time is 1-3 seconds; the stretched BOPP film needs to be air-cooled immediately, and the cold air temperature is 15-30°C;
[0033] 4) After the transverse stretching process, it goes through the online thickness measurement, edge material cutting, static elimination, automatic winding, and aging treatment production processes in sequence;
[0034] 5) Cut into finished film rolls of corresponding specifications according to requirements.
[0035] By adopting the above technical scheme, the preparation method of the present application does not require any improvement to the equipment. By setting the process parameters, the qualified rate of the prepared BOPP cosmetic film is relatively high, which can reach more than 99%. The production process is stable and controllable, and is suitable for mass production.
[0036] In summary, the present application includes at least one of the following beneficial technical effects:
[0037] 1. Adding lubricating masterbatch to the upper surface of the film is to obtain a lower friction coefficient, so that the upper surface of the film can run more smoothly when it contacts the metal surface of the packaging equipment; adding anti-sticking masterbatch is to prevent the film from becoming sticky during production or use and to improve the opening property; adding anti-static masterbatch to the core layer of the film is to effectively reduce the impact of static electricity on packaging during production, transportation, and machine operation; adding elastomers to the upper and lower surface layers of the film is to reduce the heat sealing temperature to meet customers' requirements for low-temperature heat sealing and puncture resistance, and also has a positive additive effect on improving wear resistance; the lubricating masterbatch abandons the common silicone oil in the industry, which can further improve the wear resistance of the film surface. Through the mutual synergy between the raw materials, the original wear resistance is taken to a higher level, completely achieving the same effect as POF, or even better.
[0038] 2. The room temperature friction coefficient of the BOPP cosmetic film prepared in the present application is between 0.09-0.16, the high temperature friction coefficient is between 0.11-0.20, the wear resistance is lower than 0.11%, and the lowest can reach 0.01; at the same time, its anti-puncture effect is excellent, and the lowest heat sealing temperature can reach 98°C; compared with POF film, it has obvious advantages in wear resistance, transparency, heat sealing temperature and anti-puncture effect. DETAILED DESCRIPTION
[0039] The present application is further described in detail below in conjunction with the specific contents.
[0040] raw material
[0041] The average molecular weight of the hydrolyzed polymaleic anhydride is 400; the particle size range of the nano titanium dioxide is 30-40 nm.
[0042] Preparation Example
[0043] Preparation Example 1
[0044] A nano-titanium dioxide grafted hyperbranched polymer composite material, the preparation method of which is as follows:
[0045] 1) Add 5 g of nano titanium dioxide to 32 g of xylene, disperse by ultrasonic, then add 5 g of water, 3 g of ethanol and 85 g of vinyltrimethoxysilane, adjust the pH of the system to 6, stir and react at 55° C. for 8 h to obtain silane coupling agent modified nano titanium dioxide;
[0046] 2) Add 1.5 g of hydrolyzed polymaleic anhydride, 6 g of 2-aminoterephthalic acid, 2.5 g of diisopropanolamine, 2.5 g of triethanolamine and 0.3 g of n-propyl titanate to 5 g of DMF, heat to 130° C., stir and react for 22 h to obtain a hyperbranched polymer;
[0047] 3) Under a nitrogen atmosphere, 3.5 g of silane coupling agent-modified nano-titanium dioxide was added to 7 g of DMF, and then 5 g of vinyltrimethoxysilane and 1.5 g of the hyperbranched polymer prepared in step 2) were added. After stirring for 1.5 h, 0.004 g of initiator was added, and the reaction was stirred at 75 ° C for 22 h. The reaction was filtered and dried to obtain a nano-titanium dioxide grafted hyperbranched polymer composite material.
[0048] Example
[0049] Examples 1-3
[0050] A wear-resistant and puncture-resistant BOPP cosmetic film is made by co-extrusion of an upper surface layer, a core layer and a lower surface layer. The thickness of the BOPP cosmetic film is 28 μm, the upper surface layer is 1 μm, the core layer is 26 μm, and the lower surface layer is 1 μm. The raw materials and the amounts of the raw materials of each layer are shown in Table 1. The preparation method of the BOPP cosmetic film is as follows:
[0051] 1) After the raw materials of the core layer are uniformly mixed and dried, they enter the series-connected melting single-screw extruder and metering single-screw extruder for melting and plasticization, and then pass through the coarse filter, metering pump, main filter, and enter the die head. The temperature of each section is set to 230°C and the melt temperature is 240°C;
[0052] 2) After the raw materials of the upper surface layer and the lower surface layer are mixed evenly and dried, they enter their respective single-screw extruders for melt plasticization, and then pass through a filter and a metering pump and enter the die head. The temperature of each section is set to 230°C and the melt temperature is 235°C;
[0053] 3) The three layers of polymer melt flow out after converging at the die head, and under the action of the air knife attachment device, adhere to the surface of the quench roller, and form a solid casting sheet after rapid cooling by the quench roller and the water tank, and then undergo longitudinal and transverse stretching in sequence; the longitudinal preheating temperature is 105°C, the stretching temperature is 85°C, the setting temperature is 110°C, and the longitudinal stretching ratio is 6; the transverse preheating temperature is 185°C, the stretching temperature is 145°C, the transverse stretching ratio is 9, the setting temperature is 165°C, and the time is 2 seconds; the stretched BOPP film needs to be air-cooled immediately, and the cold air temperature is 20°C;
[0054] 4) After the transverse stretching process, it goes through the online thickness measurement, edge material cutting, static elimination, automatic winding, and aging treatment production processes in sequence;
[0055] 5) Cut into finished film rolls of corresponding specifications according to requirements.
[0056] Among them, the slippery masterbatch is prepared by mixing ultra-high viscosity silicone and copolymer polypropylene in a weight ratio of 1:8, and the viscosity of the ultra-high viscosity silicone at 25°C is 500,000; the elastomer used in the upper and lower surface layers is a copolymer of propylene and butene, and the butene added during the preparation of the elastomer accounts for 5wt% of the total weight of propylene and butene; the antistatic masterbatch is prepared from homopolymer polypropylene and non-ionic glyceryl monostearate, and the mass percentage concentration of non-ionic glyceryl monostearate in the antistatic masterbatch is 15%; the anti-sticking masterbatch of the upper surface layer is prepared from copolymer polypropylene and silica, and the mass percentage concentration of the silica in the anti-sticking masterbatch is 4.5-5.5%, and the particle size of the silica is 4μm.
[0057] Table 1 Raw materials and raw material amounts of each layer of Examples 1-3 (kg)
[0058]
[0059] Example 4
[0060] A wear-resistant and puncture-resistant BOPP cosmetic film, which is different from Example 2 in that its upper surface layer also includes 1 kg of nano-titanium dioxide grafted hyperbranched polymer composite material, the nano-titanium dioxide grafted hyperbranched polymer composite material comes from Preparation Example 1, and the remaining steps are the same as Example 2.
[0061] Example 5
[0062] A wear-resistant and puncture-resistant BOPP cosmetic film, which is different from Example 2 in that its upper surface layer also includes 3 kg of nano-titanium dioxide grafted hyperbranched polymer composite material, the nano-titanium dioxide grafted hyperbranched polymer composite material comes from Preparation Example 1, and the remaining steps are the same as Example 2.
[0063] Example 6
[0064] A wear-resistant and puncture-resistant BOPP cosmetic film, which is different from Example 2 in that its upper surface layer also includes 5 kg of nano-titanium dioxide grafted hyperbranched polymer composite material, the nano-titanium dioxide grafted hyperbranched polymer composite material comes from Preparation Example 1, and the remaining steps are the same as Example 2.
[0065] Comparative Example
[0066] Comparative Example 1
[0067] A wear-resistant and puncture-resistant BOPP cosmetic film, which is different from Example 4 in that no ultra-high viscosity silicone is added to its slippery masterbatch, and the remaining steps are the same as Example 4.
[0068] Comparative Example 2
[0069] A wear-resistant and puncture-resistant BOPP cosmetic film, which is different from Example 4 in that the particle size range of nano-titanium dioxide used in the preparation of its nano-titanium dioxide grafted hyperbranched polymer composite material is 50-70nm, and the remaining steps are the same as Example 4.
[0070] Comparative Example 3
[0071] A wear-resistant and puncture-resistant BOPP cosmetic film, which is different from Example 4 in that the average molecular weight of the hydrolyzed maleic anhydride used in the preparation of its nano-titanium dioxide grafted hyperbranched polymer composite material is 800, and the amount of hydrolyzed maleic anhydride added is twice the original amount, and the remaining steps are the same as Example 4.
[0072] Comparative Example 4
[0073] The thickness of common commercially available POF film is 28 μm.
[0074] Performance testing
[0075] Detection method / test method
[0076] BOPP cosmetic films were prepared according to the preparation methods of Examples 1-6 and Comparative Examples 1-4, and then tested according to the following testing method. The test results are shown in Table 2.
[0077] Friction coefficient: tested according to the test method in GB10006-1988 (2004), the testing instrument is a peel tester, which tests the friction coefficient at room temperature (25°C) and the friction coefficient at high temperature (50°C) respectively;
[0078] Transparency: Tested according to the test method in GB / T2140-2008.
[0079] Table 2 Test results of Examples 1-6 and Comparative Examples 1-4
[0080]
[0081]
[0082] It can be seen from Examples 1-6 and Comparative Examples 1-4, as well as the test data in Table 2, that the room temperature friction coefficient of the BOPP cosmetic film prepared in the present application is between 0.09-0.16, the high temperature friction coefficient is between 0.11-0.20, the wear resistance is lower than 0.11%, and the lowest can reach 0.01; at the same time, its anti-puncture effect is excellent, and the lowest heat sealing temperature can reach 98°C; combined with Comparative Example 4, compared with the POF film, it has obvious advantages in terms of wear resistance, transparency, heat sealing temperature and anti-puncture effect.
[0083] It can be seen from the test data of Examples 1-3 of the present application that the raw material ratios of Example 2 of the present application are better; combined with Examples 4-6, it can be seen that the present application can improve the wear resistance of the BOPP cosmetic film by adding nano-titanium dioxide grafted hyperbranched polymer composite materials to the upper surface layer, and as the amount of addition increases, the wear resistance can be reduced to 0.01%, but the transparency is gradually increasing. Considering the overall effect, the comprehensive performance of the BOPP cosmetic film of Example 5 is better.
[0084] It can be seen from the test data of Example 4 and Comparative Example 1 that when ultra-high viscosity silicone is not added to the slippery masterbatch in this application, its friction coefficient is greatly improved, indicating that when only the nano-titanium dioxide grafted hyperbranched polymer composite is added, its wear resistance is poor, and there is a synergistic effect between the nano-titanium dioxide grafted hyperbranched polymer composite and the ultra-high viscosity silicone. Combined with Comparative Example 2, when the particle size of the nano-titanium dioxide in the preparation of the nano-titanium dioxide grafted hyperbranched polymer composite is large, the surface formed on the surface of the BOPP cosmetic film is easy to be uneven, which reduces the wear resistance. Combined with Comparative Example 3, when the average molecular weight of hydrolyzed maleic anhydride is large, the viscosity of the nano-titanium dioxide grafted hyperbranched polymer composite is large, which is not conducive to its dispersion in the system, so the wear resistance of the BOPP cosmetic film is low.
[0085] The above-mentioned specific implementation examples are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. Therefore, all equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A wear-resistant and puncture-resistant BOPP cosmetic film, characterized by: The BOPP cosmetic film is made of a three-layer structure consisting of an upper surface layer, a core layer and a lower surface layer, which are co-extruded and compounded; The upper surface layer comprises the following raw materials in parts by weight: 59-78 parts by weight of copolymerized polypropylene, 10-15 parts by weight of slip masterbatch, 2-6 parts by weight of anti-stick masterbatch, and 10-20 parts by weight of elastomer; the slip masterbatch is prepared by mixing ultra-high viscosity silicone and copolymerized polypropylene in a weight ratio of 1:(8-10); The core layer comprises the following raw materials in parts by weight: 96-98 parts by weight of homopolypropylene and 2-4 parts by weight of antistatic masterbatch; The lower surface layer comprises the following raw materials in parts by weight: 70-80 parts by weight of copolymerized polypropylene and 20-30 parts by weight of elastomer; The ultra-high viscosity silicone has a viscosity of 500,000-1,000,000 at 25°C; The upper surface layer further comprises 1-5 parts by weight of a nano-titanium dioxide grafted hyperbranched polymer composite material; The preparation method of the nano-titanium dioxide grafted hyperbranched polymer composite material is as follows: 1) Add 4.5-5.5 parts by weight of nano-titanium dioxide to 30-35 parts by weight of xylene, disperse by ultrasonication, then add 4-6 parts by weight of water, 2-4 parts by weight of ethanol, and 80-90 g of vinyltrimethoxysilane, adjust the pH of the system to 5-6, and stir the reaction at 50-60° C. for 7-9 hours to obtain silane coupling agent-modified nano-titanium dioxide; the particle size of the nano-titanium dioxide is in the range of 30-40 nm; 2) Adding 1-2 parts by weight of hydrolyzed polymaleic anhydride, 5-7 parts by weight of 2-aminoterephthalic acid, 2-3 parts by weight of diisopropanolamine, 2-3 parts by weight of triethanolamine, and 0.25-0.35 parts by weight of n-propyl titanate to 5-6 parts by weight of DMF, heating to 125-135° C., and stirring for 20-24 hours to obtain a hyperbranched polymer; 3) Under a nitrogen atmosphere, adding 3-4 parts by weight of a silane coupling agent-modified nano-titanium dioxide to 6-8 parts by weight of DMF, then adding 4-6 parts by weight of vinyltrimethoxysilane and 1-2 parts by weight of the hyperbranched polymer prepared in step 2), stirring for 1-2 hours, adding 0.003-0.005 parts by weight of an initiator, stirring at 70-80° C. for 20-24 hours, filtering, and drying to obtain a nano-titanium dioxide grafted hyperbranched polymer composite material; The average molecular weight of the hydrolyzed polymaleic anhydride is 400; The elastomer used in the upper surface layer and the lower surface layer is a copolymer of propylene and butene. The butene added during the preparation of the elastomer accounts for 5-10 wt % of the total weight of propylene and butene.
2. The wear-resistant and puncture-resistant BOPP cosmetic film according to claim 1, characterized in that: The antistatic masterbatch is prepared from homopolypropylene and nonionic glyceryl monostearate, and the mass percentage concentration of nonionic glyceryl monostearate in the antistatic masterbatch is 15%.
3. The wear-resistant and puncture-resistant BOPP cosmetic film according to claim 1, characterized in that: The upper surface anti-sticking masterbatch is made of copolymerized polypropylene and silicon dioxide. The mass percentage concentration of the silicon dioxide in the anti-sticking masterbatch is 4.5-5.5%, and the particle size of the silicon dioxide is 4 μm.
4. The wear-resistant and puncture-resistant BOPP cosmetic film according to claim 1, characterized in that: The thickness of the BOPP cosmetic film is 28 μm, the upper surface layer is 1-1.5 μm, the core layer is 25-26 μm, and the lower surface layer is 1-1.5 μm.
5. A method for preparing a wear-resistant and puncture-resistant BOPP cosmetic film according to any one of claims 1 to 4, characterized in that: It comprises the following preparation steps: 1) After the raw materials of the core layer are uniformly mixed and dried, they are fed into a melting single-screw extruder and a metering single-screw extruder connected in series for melt plasticization. The extruder then passes through a coarse filter, a metering pump, and a main filter before entering the die head. The temperature of each section is set at 220-250°C, and the melt temperature is 210-270°C. 2) The raw materials of the upper surface layer and the lower surface layer are mixed uniformly and dried, and then enter respective single-screw extruders for melt plasticization. The raw materials then pass through a filter and a metering pump before entering a die head. The temperature of each section is set at 220-240°C, and the melt temperature is set at 220-250°C. 3) The three layers of polymer melt flow out after converging at the die head. Under the action of the air knife attachment device, they adhere to the surface of the chill roller. After rapid cooling by the chill roller and water tank, a solid casting sheet is formed. It is then stretched in the longitudinal and transverse directions in sequence. The longitudinal preheating temperature is 95-125℃, the stretching temperature is 70-100℃, the setting temperature is 80-130℃, and the longitudinal stretch ratio is 5.0-7.5; the transverse preheating temperature is 170-200℃, the stretching temperature is 130-160℃, the transverse stretch ratio is 8-10, the setting temperature is 155-175℃, and the time is 1-3 seconds. The stretched BOPP film needs to be immediately air-cooled, and the cold air temperature is 15-30℃. 4) After the transverse stretching process, it goes through the online thickness measurement, edge material cutting, static elimination, automatic winding, and aging treatment production processes in sequence; 5) Cut into finished film rolls of corresponding specifications as required.
Citation Information
Patent Citations
Low-temperature heat-seal shrinking packaging film used for cigarettes and manufacturing method thereof
CN105619990A
High-temperature resistance wear-resistant BOPP film used for cigarettes, and preparation method thereof