Environmentally friendly recycled concrete and its preparation process

By using activators and carbon dioxide reaction in recycled concrete to consume unhydrated cementitious materials, combined with the use of waterproofing agents, the problem of increased alkalinity and expansion in recycled concrete is solved, and the preparation of environmentally friendly recycled concrete is realized, which reduces the alkali Aggregate reaction and swelling risk.

CN116102316BActive Publication Date: 2024-10-18NANTONG JIANSHE CONCRETE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310108021.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-14
Publication Date
2024-10-18
Estimated Expiration
2043-02-14

AI Technical Summary

Technical Problem

The unhydrated cementitious material of recycled coarse aggregate in existing recycled concrete causes the alkalinity of the concrete mixture to increase, which increases the risk of alkali-aggregate reaction and easily causes concrete expansion.

Method used

By using an activator in the first modification liquid to stimulate the hydration activity of waste concrete particles, and in the second modification liquid to promote the reaction between calcium hydroxide and carbon dioxide, the unhydrated cementitious materials are consumed and the alkali of the concrete mixture is reduced. degree, while using waterproofing agents to reduce humidity and limit the diffusion of alkaline components.

Benefits of technology

It effectively reduces the alkalinity of the concrete mixture, reduces the alkali-aggregate reaction, alleviates the expansion of recycled concrete, and achieves carbon neutrality, energy conservation and environmental protection through carbon dioxide fixation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004075718390000061
    Figure BDA0004075718390000061
Patent Text Reader

Abstract

The present application relates to the field of concrete technology, and specifically discloses an environmentally friendly recycled concrete and a preparation process thereof. Environmentally friendly recycled concrete is obtained by concrete mixture after mold curing, and the concrete mixture includes the following components by weight: 1160-1180 parts of recycled coarse bone, 780-800 parts of fine aggregate, 36-40 parts of waterproofing agent, 250-270 parts of Portland cement, 100-120 parts of fly ash, 118-122 parts of water, and 3.5-3.9 parts of water reducer. The present application stimulates the hydration activity of waste concrete particles by an activator, and then promotes the carbonization of waste concrete particles by a second modified liquid, consumes the cementitious materials remaining in the waste concrete particles, and obtains recycled coarse aggregate. The recycled coarse aggregate of the present application is not easy to release calcium hydroxide in the concrete mixture, so the alkalinity of the concrete mixture is reduced compared with the case of directly using waste concrete particles, which helps to alleviate the alkali-aggregate reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of concrete, and more specifically, to an environmentally friendly recycled concrete and a preparation process thereof. Background Art

[0002] Recycled aggregate refers to the aggregate obtained by crushing construction waste such as waste concrete and waste clay bricks, and then screening, cleaning, etc. Using recycled aggregate to produce recycled concrete is one of the reasonable ways to dispose of construction waste, which can reduce the consumption of natural aggregates and reduce damage to the environment.

[0003] In the related art, there is a recycled concrete, which is obtained by curing a concrete mixture into a mold. The concrete mixture includes the following components in parts by weight: 1170 parts of recycled coarse aggregate, 790 parts of fine aggregate, 260 parts of Portland cement, 110 parts of fly ash, 120 parts of water, and 3.7 parts of a water reducer. The fine aggregate is quartz sand, and the recycled coarse aggregate is a crushed product of waste concrete.

[0004] With respect to the above-mentioned related technologies, the inventors believe that in the related technologies, a part of unhydrated cementitious material is still retained in the particles of the recycled coarse aggregate. After this part of cementitious material is hydrated in the concrete mixture, the alkalinity of the concrete mixture will increase, and there is a risk of aggravating the alkali-aggregate reaction, which can easily cause the expansion of the concrete. Summary of the invention

[0005] In the related art, recycled coarse aggregate will increase the alkalinity of the concrete mixture, thereby intensifying the alkali-aggregate reaction and easily causing the expansion of the concrete. In order to improve this defect, the present application provides an environmentally friendly recycled concrete and a preparation process thereof.

[0006] In the first aspect, the present application provides an environmentally friendly recycled concrete, which adopts the following technical solution:

[0007] The invention discloses an environmentally friendly recycled concrete, wherein the environmentally friendly recycled concrete is obtained by curing a concrete mixture into a mold, wherein the concrete mixture comprises the following components in parts by weight: 1160-1180 parts of recycled coarse aggregate, 780-800 parts of fine aggregate, 36-40 parts of waterproofing agent, 250-270 parts of Portland cement, 100-120 parts of fly ash, 118-122 parts of water, and 3.5-3.9 parts of water reducing agent. The recycled coarse aggregate is obtained by soaking waste concrete particles in a first modifying liquid and a second modifying liquid in sequence, wherein the components of the first modifying liquid include water and an activator, wherein the activator is used to activate the hydration activity of the waste concrete particles, wherein the components of the second modifying liquid include water, carbon dioxide and propylene carbonate, wherein the weight ratio of water to propylene carbonate in the second modifying liquid is 1:(0.9-1.1), and the carbon dioxide is in a saturated dissolved state in the second modifying liquid.

[0008] By adopting the above technical scheme, the present application performs preliminary modification on the waste concrete particles through the first modifying liquid, and the activator in the first modifying liquid activates the waste concrete particles, prompting the unhydrated cementitious materials in the waste concrete particles to react with water, and converting the unhydrated cementitious materials into calcium hydroxide. Then, after being treated with the second modifying liquid, the calcium hydroxide reacts with carbon dioxide, completes further carbonization, and obtains the regenerated coarse aggregate. The regenerated coarse aggregate of the present application is continuously treated with the first modifying liquid and the second modifying liquid, which consumes the unhydrated cementitious materials, reduces the amount of calcium hydroxide produced in the concrete mixture, reduces the alkalinity of the concrete mixture, helps to alleviate the alkali-aggregate reaction, and alleviates the expansion of the recycled concrete. In addition, the waterproofing agent can reduce the internal humidity of the concrete, limit the diffusion of the alkaline components, and also help to inhibit the alkali-aggregate reaction.

[0009] When the source of carbon dioxide is industrial carbon dioxide tail gas, using propylene carbonate to absorb carbon dioxide is one of the optional treatment methods. The present application uses a mixture of water and propylene carbonate to absorb carbon dioxide, which provides reaction conditions for the reaction of carbon dioxide and calcium hydroxide by adding water, realizes the fixation of carbon dioxide, and is also an optimization of the treatment method of carbon dioxide tail gas.

[0010] Preferably, the concrete mixture comprises the following components in parts by weight: 1165-1175 parts of recycled coarse aggregate, 785-795 parts of fine aggregate, 37-39 parts of waterproofing agent, 255-265 parts of Portland cement, 105-115 parts of fly ash, 119-121 parts of water, and 3.6-3.8 parts of water reducing agent.

[0011] By adopting the above technical solution, the raw material ratio of the concrete mixture is optimized, which is helpful to suppress the alkali-aggregate reaction.

[0012] Preferably, the recycled coarse aggregate is prepared according to the following method:

[0013] (1) crushing waste concrete to obtain waste concrete particles; mixing water and an activator to obtain a first modified liquid; mixing water and propylene carbonate, and then introducing carbon dioxide to saturation to obtain a second modified liquid;

[0014] (2) mixing the waste concrete particles and the first modified liquid, immersing them under negative pressure for 40-60 minutes, and then filtering and recovering the waste concrete particles;

[0015] (3) The recycled waste concrete particles are put into the second modified liquid and stirred for 4-5 hours. During the immersion process, carbon dioxide is continuously introduced into the second modified liquid. After the immersion is completed, the particles are filtered and dried to obtain recycled coarse aggregate.

[0016] By adopting the above technical scheme, the present application first uses a first modifying liquid to impregnate the waste concrete particles under negative pressure conditions, so that the activator in the first modifying liquid fully enters the pores of the waste concrete particles and activates the waste concrete particles, and then consumes the calcium hydroxide produced by the activation through the treatment of the second modifying liquid to obtain recycled coarse aggregate.

[0017] Preferably, the first modifying liquid further comprises sodium carbonate.

[0018] By adopting the above technical solution, when the cementitious material remaining in the waste concrete particles undergoes a hydration reaction, the generated calcium hydroxide reacts with sodium carbonate to produce calcium carbonate and sodium hydroxide. Sodium hydroxide is easily soluble in water, and therefore easily dissolves from the waste concrete particles, which is equivalent to consuming the components with hydration activity in the waste concrete particles in advance, reducing the alkalinity of the concrete mixture, and helping to alleviate the alkali-aggregate reaction. In addition, sodium hydroxide can promote the breaking of the silicon-oxygen bonds and aluminum-oxygen bonds of the residual cementitious material in the waste concrete particles, thereby increasing the reaction activity of the residual cementitious material, promoting the full release of the hydration activity of the waste concrete particles, reducing the alkalinity of the concrete mixture, and helping to alleviate the alkali-aggregate reaction.

[0019] Preferably, the stimulator is triethanolamine.

[0020] By adopting the above technical solution, triethanolamine can promote the hydration reaction of tricalcium aluminate phase in the remaining cement particles in the waste concrete particles, and the nitrogen atoms in triethanolamine are easy to complex with the metal ions in the waste concrete particles, which is conducive to accelerating the diffusion rate of hydration products and achieving the excitation and activation effect on the waste concrete particles. The excitation effect of triethanolamine increases the total amount of calcium hydroxide generated during the impregnation process, consumes the components with hydration activity in the waste concrete particles in advance, helps to reduce the alkalinity of the concrete mixture, and alleviates the alkali-aggregate reaction in the recycled concrete.

[0021] Preferably, the activator is calcium chloride.

[0022] By adopting the above technical solution, calcium ions and chloride ions ionized from calcium chloride can diffuse into the vitreous phase in the waste concrete, and react with the alumina components in the vitreous phase to produce hydrated calcium chloroaluminate, thereby stimulating the activity of the waste concrete particles. At the same time, calcium chloride can also react with calcium hydroxide to produce calcium oxychloride complex salt, thereby consuming calcium hydroxide, consuming the components with hydration activity in the waste concrete particles in advance, and alleviating the alkali-aggregate reaction in the recycled concrete.

[0023] Preferably, in step (2) of preparing the recycled coarse aggregate, the vacuum degree under negative pressure conditions is 140-200 mbar.

[0024] By adopting the above technical scheme, the vacuum degree under negative pressure conditions is optimized. At a vacuum degree of 140-200 mbar, the activator can easily penetrate into the waste concrete particles. When the vacuum degree is higher than 200 mbar, the penetration effect of the activator is not ideal, and when the vacuum degree is lower than 140 mbar, the penetration effect of the activator does not increase significantly.

[0025] Preferably, the waterproofing agent comprises sodium silicate.

[0026] By adopting the above technical solution, sodium silicate can form a waterproof film in concrete to hinder the penetration of water. At the same time, sodium silicate can react with calcium hydroxide produced by the hydration of silicate cement to produce calcium silicate, which helps to reduce the alkalinity of concrete and helps to alleviate alkali-aggregate reaction.

[0027] Preferably, the waterproofing agent further comprises dodecyltriethoxysilane.

[0028] By adopting the above technical solution, dodecyltriethoxysilane can be hydrolyzed in the concrete mixture and dodecyl can be grafted on the surface of cement particles, which enhances the hydrophobicity of the cement particles, enhances the waterproof effect, and helps to alleviate the alkali-aggregate reaction.

[0029] In a second aspect, the present application provides a process for preparing an environmentally friendly recycled concrete, which adopts the following technical solution.

[0030] A process for preparing environmentally friendly recycled concrete comprises the following steps:

[0031] (1) mixing water and a water reducing agent to obtain a water reducing agent solution; mixing recycled coarse aggregate, fine aggregate, a waterproofing agent, silicate cement and fly ash to obtain a dry material;

[0032] (2) mixing the dry material and the water reducing agent solution, and stirring to obtain a concrete mixture;

[0033] (3) The concrete mixture is placed into a mold for curing, and environmentally friendly recycled concrete is obtained after reaching a specified age.

[0034] By adopting the above technical solution, the method of the present application prepares dry materials and water reducing agent solution respectively, and then obtains a concrete mixture after mixing the dry materials and the water reducing agent solution. After the concrete mixture is put into a mold for curing, an environmentally friendly recycled concrete is obtained. The environmentally friendly recycled concrete of the present application fixes carbon dioxide through recycled coarse aggregate, which helps to achieve carbon neutrality and energy conservation and environmental protection.

[0035] In summary, this application has the following beneficial effects:

[0036] 1. The present application stimulates the hydration activity of waste concrete particles by an activator, and then promotes the carbonization of waste concrete particles by a second modified liquid, consumes the residual cementitious materials in the waste concrete particles, and obtains recycled coarse aggregate. The recycled coarse aggregate of the present application is not easy to release calcium hydroxide in the concrete mixture, so compared with the case of directly using waste concrete particles, the alkalinity of the concrete mixture is reduced, which helps to alleviate the alkali-aggregate reaction and reduce the expansion of recycled concrete.

[0037] 2. In the present application, calcium chloride is preferably used as the activator. Calcium chloride can stimulate the activity of waste concrete particles. At the same time, calcium chloride can also react with calcium hydroxide to produce calcium oxychloride complex salt, thereby consuming calcium hydroxide, consuming the components with hydration activity in the waste concrete particles in advance, and alleviating the alkali-aggregate reaction in the recycled concrete. DETAILED DESCRIPTION

[0038] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.

[0039] Preparation example of recycled coarse aggregate

[0040] The following is an explanation using Preparation Example 1.

[0041] Preparation Example 1

[0042] In this preparation example, the recycled coarse aggregate is prepared according to the following method:

[0043] (1) crushing 1400 kg of waste concrete with strength grade C40 to obtain waste concrete particles; mixing 1000 kg of water, 30 kg of sodium carbonate, and 10 kg of an activator to obtain a first modified liquid; mixing 500 kg of water and 500 kg of propylene carbonate, and then introducing carbon dioxide into the mixture until saturated to obtain a second modified liquid; in this step, the activator is triethanolamine;

[0044] (2) mixing the waste concrete particles and the first modified liquid, immersing them under a negative pressure condition of 220 mbar for 45 minutes, and then filtering and recovering the waste concrete particles;

[0045] (3) The recovered waste concrete particles are put into the second modified liquid and stirred for 4.5 hours. Carbon dioxide is continuously introduced during the impregnation process to maintain the carbon dioxide in the second modified liquid at a saturated state. After the impregnation is completed, the particles are filtered and dried at 105° C. to obtain recycled coarse aggregate.

[0046] Preparation Example 2

[0047] The difference between this preparation example and preparation example 1 is that calcium chloride is used as the activator.

[0048] Preparation Example 3-6

[0049] As shown in Table 1, the difference between Preparation Examples 3-6 and Preparation Example 1 is that, in step (2) of preparing recycled coarse aggregate, the vacuum degree under negative pressure conditions is different.

[0050] Table 1 Vacuum degree under negative pressure conditions

[0051] sample Preparation Example 1 Preparation Example 3 Preparation Example 4 Preparation Example 5 Preparation Example 6 Vacuum degree / mbar 220 200 170 140 120

[0052] Preparation Example 7

[0053] The difference between this preparation example and preparation example 1 is that the components of the first modifying liquid do not include an activator.

[0054] Preparation Example 8

[0055] This preparation example is different from preparation example 1 in that the components of the first modifying liquid do not include sodium carbonate.

[0056] Example

[0057] Examples 1-5

[0058] The following description is given by taking Example 1 as an example.

[0059] Example 1

[0060] In this embodiment, recycled coarse aggregate is prepared according to the method of Preparation Example 1, fine aggregate is natural quartz sand of Zone 2 that meets the requirements of "GB / T 14684-2011 Construction Sand", the model of silicate cement is P.O42.5, fly ash is Class I fly ash produced by thermal power plants, the average molecular weight of polycarboxylate water reducer is 58000, water meets the requirements of "JGJ 63-2006 Concrete Water Standard", and the production process of concrete complies with the requirements of "GB 50164-2011 Concrete Quality Control Standard".

[0061] In this embodiment, the environmentally friendly recycled concrete is prepared according to the following steps:

[0062] (1) 122 kg of water and 3.5 kg of a water reducing agent are mixed to obtain a water reducing agent solution; 1160 kg of recycled coarse aggregate, 780 kg of fine aggregate, 36 kg of a waterproofing agent, 250 kg of silicate cement and 100 kg of fly ash are mixed to obtain a dry material; in this step, the waterproofing agent is sodium silicate;

[0063] (2) mixing the dry material and the water reducing agent solution, and stirring to obtain a concrete mixture;

[0064] (3) The concrete mixture is placed into a mold for curing, and environmentally friendly recycled concrete is obtained after reaching a specified age.

[0065] As shown in Table 1, the differences between Examples 1-5 are mainly in the different raw material ratios.

[0066] Table 1

[0067]

[0068] Embodiment 6-10

[0069] As shown in Table 2, the difference between Examples 6-10 and Example 3 is that the preparation examples of the recycled coarse aggregate are different.

[0070] Table 2 Preparation example of recycled coarse aggregate

[0071] sample Example 3 Example 6 Example 7 Example 8 Example 9 Example 10 Preparation Example Preparation Example 1 Preparation Example 2 Preparation Example 3 Preparation Example 4 Preparation Example 5 Preparation Example 6

[0072] Embodiment 11

[0073] The difference between this embodiment and embodiment 3 is that the waterproofing agent is formed by mixing sodium silicate and dodecyltriethoxysilane in a weight ratio of 20:1.

[0074] Comparative Example

[0075] Comparative Example 1

[0076] In this comparative example, the fine aggregate is natural quartz sand of Zone 2 that meets the requirements of "GB / T 14684-2011 Construction Sand", the recycled coarse aggregate is the crushed product of C40 waste concrete, and the particle size of the recycled coarse aggregate meets the continuous gradation of 5-31.5 mm. The model of silicate cement is P.O42.5, the fly ash is Class I fly ash produced by a thermal power plant, the average molecular weight of the polycarboxylate water reducer is 58000, the water meets the requirements of "JGJ 63-2006 Concrete Water Standard", and the production process of concrete meets the requirements of "GB 50164-2011 Concrete Quality Control Standard".

[0077] This comparative example provides a recycled concrete, which is obtained by curing a concrete mixture into a mold. The concrete mixture includes the following components in parts by weight: 1170 kg of recycled coarse aggregate, 790 kg of fine aggregate, 260 kg of Portland cement, 110 kg of fly ash, 120 kg of water, and 3.7 kg of a water reducer.

[0078] Comparative Example 2

[0079] This comparative example is different from Example 3 in that the components of the concrete mixture do not include a waterproofing agent.

[0080] Comparative Example 3

[0081] The difference between this comparative example and Example 3 is that the recycled coarse aggregate is prepared according to the method of Preparation Example 7.

[0082] Comparative Example 4

[0083] The difference between this comparative example and Example 3 is that the recycled coarse aggregate is prepared according to the method of Preparation Example 8.

[0084] Performance testing methods

[0085] The concrete mixture of each embodiment and comparative example was used as raw material, and mold forming and curing were carried out according to “SL / T 352-2020-3.39 Test of Alkali Activity of Aggregate (Concrete Prism Method)”, and the expansion rate was calculated according to the initial length of the sample and the length measured at 52 weeks of age. The expansion rate results of each embodiment and comparative example are the average values ​​of the measured results of 5 test pieces.

[0086] After the expansion rate is obtained, the ratio of the expansion rate of the samples of each embodiment and comparative example to the expansion rate of the sample of comparative example 1 is calculated, and the result is recorded as the relative expansion rate. The results are shown in Table 3.

[0087] Table 3 Relative expansion rate

[0088] sample Relative expansion rate / % sample Relative expansion rate / % Example 1 76.4 Example 9 75.0 Example 2 76.3 Example 10 75.0 Example 3 76.2 Embodiment 11 72.7 Example 4 76.2 Comparative Example 1 100.0 Example 5 76.1 Comparative Example 2 84.3 Example 6 74.6 Comparative Example 3 94.3 Example 7 75.4 Comparative Example 4 89.2 Example 8 75.1 / /

[0089] Combining Examples 1-5 and Comparative Example 1 and Table 3, it can be seen that the relative expansion rates measured in Examples 1-5 are less than those in Comparative Example 1, indicating that the degree of alkali-aggregate reaction in the environmentally friendly recycled concrete of the present application is equivalent to that in Comparative Example 1, and therefore the expansion of the concrete specimen is reduced.

[0090] Combining Example 3 and Comparative Example 2 and Table 3, it can be seen that the relative expansion rate measured in Example 3 is less than that in Comparative Example 2, indicating that the waterproofing agent in Example 3 inhibits the alkali-aggregate reaction by hindering the diffusion of water, thereby reducing the expansion.

[0091] Combining Example 3 and Comparative Example 3 and Table 3, it can be seen that the relative expansion rate measured in Example 3 is less than that in Comparative Example 3, indicating that in the absence of an activator, the degree of hydration of the waste concrete particles themselves is low and insufficient to consume sufficient residual cementitious materials. The residual cementitious materials increase the alkalinity after hydration, which still aggravates the alkali-aggregate reaction and causes more serious expansion.

[0092] Combining Example 3 and Comparative Example 4 and Table 3, it can be seen that the relative expansion rate measured in Example 3 is less than that in Comparative Example 4, indicating that when sodium carbonate is not added, the carbonization degree of the waste concrete particles is low and the residual calcium hydroxide may still aggravate the alkali-aggregate reaction.

[0093] Combining Example 3 and Example 6 and Table 3, it can be seen that the relative expansion rate measured in Example 6 is smaller than that in Example 3, indicating that using calcium chloride as an activator can achieve a better activating effect.

[0094] It can be seen from Example 3, Examples 7-10 and Table 3 that the activator easily penetrates into the waste concrete particles at a vacuum degree of 140-200 mbar, the penetration effect of the activator is not ideal when the vacuum degree is higher than 200 mbar, and the penetration effect of the activator is not significantly increased when the vacuum degree is lower than 140 mbar. Therefore, the vacuum degree is preferably 140-200 mbar.

[0095] It can be seen from Example 3, Example 11 and Table 3 that when sodium silicate and dodecyltriethoxysilane are used together, the inhibitory effect on the alkali-aggregate reaction can be further improved, thereby reducing the expansion rate.

[0096] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An environmentally friendly recycled concrete, characterized in that: The environmentally friendly recycled concrete is obtained by curing a concrete mixture into a mold. The concrete mixture includes the following components in parts by weight: 1165-1175 parts of recycled coarse aggregate, 785-795 parts of fine aggregate, 37-39 parts of waterproofing agent, 255-265 parts of Portland cement, 105-115 parts of fly ash, 119-121 parts of water, and 3.6-3.8 parts of water reducer. The recycled coarse aggregate is obtained by soaking waste concrete particles in a first modifying liquid and a second modifying liquid in sequence. The components of the first modifying liquid include water, an activator and sodium carbonate. The activator is triethanolamine, and the activator is used to activate the hydration activity of the waste concrete particles. The components of the second modifying liquid include water, carbon dioxide and propylene carbonate. The weight ratio of water to propylene carbonate in the second modifying liquid is 1: (0.9-1.1), and the carbon dioxide is in a saturated state of dissolution in the second modifying liquid. The recycled coarse aggregate is prepared according to the following method: (1) crushing waste concrete to obtain waste concrete particles; mixing water and an activator to obtain a first modified liquid; mixing water and propylene carbonate, and then introducing carbon dioxide to saturation to obtain a second modified liquid; (2) mixing the waste concrete particles and the first modified liquid, immersing them under negative pressure for 40-60 minutes, and then filtering and recovering the waste concrete particles; (3) The recycled waste concrete particles are put into the second modified liquid and stirred for 4-5 hours. During the impregnation process, carbon dioxide is continuously introduced into the second modified liquid. After the impregnation is completed, the particles are filtered and dried to obtain recycled coarse aggregate.

2. The environmentally friendly recycled concrete according to claim 1, characterized in that: The activator may also be replaced by calcium chloride instead of triethanolamine.

3. The environmentally friendly recycled concrete according to claim 1, characterized in that: In the step (2) of preparing the recycled coarse aggregate, the vacuum degree under negative pressure conditions is 140-200 mbar.

4. The environmentally friendly recycled concrete according to claim 1, characterized in that: The components of the waterproofing agent include sodium silicate.

5. The environmentally friendly recycled concrete according to claim 4, characterized in that: The components of the waterproofing agent also include dodecyltriethoxysilane.

6. The process for preparing the environmentally friendly recycled concrete according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) mixing water and a water reducing agent to obtain a water reducing agent solution; mixing recycled coarse aggregate, fine aggregate, a waterproofing agent, silicate cement and fly ash to obtain a dry material; (2) Mixing the dry material and the water reducing agent solution and stirring to obtain a concrete mixture; (3) The concrete mixture is placed into a mold for curing, and environmentally friendly recycled concrete is obtained after reaching a specified age.

Citation Information

Patent Citations

  • Method for preparing carbonized recycled aggregate with function of inhibiting alkali-aggregate reaction

    CN108793797A

  • C30 recycled aggregate concrete and preparation method thereof

    CN115490464A