Chiral organoboron catalyst and preparation method thereof, and application thereof in preparing optically active polycarbonate or polyester

By catalyzing the copolymerization of alkylene oxides with carbon dioxide or cyclic acid anhydrides using chiral organoboron catalysts, the problems of complex synthesis and poor performance of metal catalysts are solved, and the preparation of optically active polycarbonates and polyesters with controllable molecular weights is achieved, improving its potential for application in many fields.

CN116102726BInactive Publication Date: 2024-10-25DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310283775.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing chiral metal catalysts have cumbersome synthesis steps, poor water/oxygen tolerance, and metal residue problems when preparing optically active polycarbonates and polyesters, which limit their application in electronic products and biomedical fields, and the resulting polymers Carbonate and polyester have random structures and poor thermodynamic and mechanical properties.

Method used

A class of chiral organoboron catalysts, including organoboron-onium salt bifunctional catalysts and organoboronium salt bifunctional catalysts and two-component catalysts composed of organoboron and onium salts, were developed through specific synthesis reaction equations and steps for catalyzing alkylene oxides and carbon dioxide. Or asymmetric copolymerization of cyclic acid anhydrides to achieve the preparation of polycarbonates and polyesters with controllable molecular weight and narrow molecular weight distribution.

Benefits of technology

Efficient catalytic reaction in a wide temperature range, high catalyst activity, high selectivity of polymer products, controllable molecular weight, adjustable polymer structure, and no metal residue, expanding the application of polycarbonate and polyester in the fields of food packaging and medical materials application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004138954400000031
    Figure BDA0004138954400000031
  • Figure BDA0004138954400000032
    Figure BDA0004138954400000032
  • Figure BDA0004138954400000033
    Figure BDA0004138954400000033
Patent Text Reader

Abstract

The present invention belongs to the field of polymer materials, and in particular to a class of chiral organoboron catalysts and preparation methods thereof, and applications in the preparation of optically active polycarbonates or polyesters. Chiral organoboron catalysts include organoboron-onium salt bifunctional catalysts and organoboron and onium salt bicomponent catalysts, wherein the organoboron-onium salt bifunctional catalyst is an organoboron Lewis acid center and a Lewis base onium salt assembled into an axial chiral binaphthyl skeleton to form a bifunctional catalyst; the organoboron and onium salt bicomponent catalyst is a main catalyst formed by introducing the organoboron Lewis acid center into a chiral skeleton, and a co-catalyst salt is used as a bicomponent catalyst. The benefits of the present invention are low catalyst dosage, high activity, controllable molecular weight and narrow distribution, wide operating temperature range, and adjustable polymer structure. In addition, since there is no metal residue in the polymer, the application of polycarbonate and polyester in the fields of food packaging and medical materials will be greatly expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a chiral organic boron catalyst and a preparation method thereof, and application of the catalyst in the preparation of optically active polycarbonate or polyester. Background Art

[0002] Polycarbonate and polyester are widely used in the automotive industry, biomedicine, food packaging, electrochemistry and other fields. Compared with other methods for synthesizing polycarbonate and polyester, the copolymerization of alkylene oxide with carbon dioxide or cyclic anhydride is not only atom-economical, but also has a wide variety of alkylene oxides, and copolymers with different structures can be synthesized. Therefore, the preparation of polycarbonate and polyester by copolymerization reaction involving alkylene oxide has attracted widespread attention in recent years.

[0003] At present, chiral metal catalysts have achieved high enantioselectivity in catalyzing the desymmetric copolymerization of alkylene oxides with carbon dioxide or cyclic anhydrides, such as bimetallic Salen Co (III) complexes based on biphenyl bridges (CN 103102480B), bimetallic Salen Al complexes based on biphenyl or binaphthyl bridges (CN 106117532 B), and bimetallic bifunctional Salen Al complexes based on binaphthyl or hydrogenated binaphthyl bridges (CN 114163627 A), which are used to catalyze the desymmetric copolymerization of alkylene oxides and successfully prepare polycarbonates or polyesters with perfect isotactic structures. However, the synthesis steps of metal complexes are generally cumbersome, and the tolerance to water / oxygen is poor. In addition, metal residues usually make polycarbonates and polyesters colored and toxic, and the complete removal of toxic metal residues is still a difficult challenge, thus hindering their application in electronic products and biomedicine.

[0004] In the past two decades, organic catalysts have been widely used in the field of organic synthesis due to their advantages such as low cost, easy availability and no toxic metal residues. In 2016, Feng et al. first reported that the triethylborane / PPNCl catalytic system achieved the alternating copolymerization of alkylene oxide and carbon dioxide (J.Am.Chem.Soc.2016,138,11117-11120). Subsequently, Meng Yuezhong's research group (CN 109679077 B) used commercial (thio)urea / organic base to catalyze the ring-opening copolymerization of alkylene oxide and cyclic anhydride to prepare polyester. This polymerization not only has a high catalytic activity (TOF up to 456h -1) and product selectivity (>99% polyester selectivity), and reduced the production cost of polyester, expanding its application prospects in biodegradable materials. Tao Youhua's research group (CN114605621A) designed a class of hydrogen-bond donor-boron organic catalysts that are easy to synthesize and can be modularly adjusted. This type of catalyst also shows high catalytic activity in the ring-opening copolymerization of alkylene oxides and cyclic anhydrides (TOF value up to 408h -1 ) and product selectivity (>99% polyester selectivity). It is worth noting that Wu Guangpeng's research group reported a series of electrophilic-nucleophilic bifunctional catalysts based on organoboron, which have extremely high activity in catalyzing the copolymerization of alkylene oxides, achieving a conversion efficiency of 5.0 kg polycarbonate / g catalyst and 7.4 kg polyester / g catalyst (CN 110938087 B, CN113087882 A, CN 112387307B).

[0005] Although the organic catalysts reported in the above patents show very excellent catalytic activity in the copolymerization reaction involving alkylene oxides, the resulting polycarbonate and polyester are both random structures, and random polycarbonate and polyester materials show relatively poor thermodynamic and mechanical properties, which limits their practical applications in various fields. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a class of chiral organoboron catalysts and their application in efficiently catalyzing the asymmetric copolymerization reaction of alkylene oxides with carbon dioxide or cyclic anhydrides, so as to realize the preparation of polycarbonates and polyesters with controllable molecular weight and narrow molecular weight distribution within a wide temperature range. At the same time, the prepared copolymers have moderate enantioselectivity and are optically active polycarbonate and polyester materials.

[0007] The technical solution of the present invention is as follows:

[0008] A chiral organoboron catalyst, the chiral organoboron catalyst includes an organoboron-onium salt bifunctional catalyst and a bicomponent catalyst composed of an organoboron and an onium salt; wherein the organoboron-onium salt bifunctional catalyst is a bifunctional catalyst formed by assembling an organoboron Lewis acid center and a Lewis base onium salt into an axially chiral binaphthyl skeleton; the bicomponent catalyst composed of an organoboron and an onium salt is a main catalyst formed by introducing an organoboron Lewis acid center into a chiral skeleton, and a cocatalyst The general structural formula of the organic boron-onium salt dual-functional catalyst and the organic boron and onium salt dual-component catalyst is as follows:

[0009]

[0010] In the formula, the specific structure of the organic boron-onium salt bifunctional catalyst is:

[0011]

[0012] The specific structure of the main catalyst of the organic boron and onium salt two-component catalyst is:

[0013]

[0014] Cocatalyst for organic boron-onium salt two-component catalyst The salt is bis(triphenylphosphine)-imino chloride (PPNCl), and its specific structure is:

[0015]

[0016] In the class of chiral organoboron catalysts, the synthesis reaction equation of the bifunctional catalyst 1 is:

[0017]

[0018] The specific preparation steps of the bifunctional catalyst 1 are:

[0019] Under the protection of inert gas, (R)-2,2'-bis(bromomethyl)-1,1'-binaphthyl, K2CO3 and diallylamine in a molar ratio of 1:2:1 are mixed, dissolved in acetonitrile, refluxed at 90-150°C for 6-10 hours, and then water is added to quench the reaction. The organic phase is separated, the aqueous phase is extracted with an organic solvent, and the solvent is removed under reduced pressure to obtain a crude product. The crude product is purified by column chromatography to obtain a chiral ammonium salt of axial binaphthyl. Under the protection of inert gas, 9-boranebicyclo[3.3.1]nonane and a tetrahydrofuran solution of a chiral ammonium salt of axial binaphthyl are mixed, wherein the molar ratio of 9-boranebicyclo[3.3.1]nonane to the chiral ammonium salt of axial binaphthyl is 2:1, and then reacted at 40-60°C for 2-12 hours, filtered, and the filter cake is washed with n-hexane for multiple times, and vacuum dried to obtain a bifunctional catalyst 1.

[0020] In the class of chiral organoboron catalysts, the synthesis reaction equation of bifunctional catalyst 2 is:

[0021]

[0022] The specific preparation steps of bifunctional catalyst 2 are:

[0023] Under the protection of inert gas, (R)-2,2'-bis(bromomethyl)-1,1'-binaphthyl, K2CO3 and N-methylallylamine in a molar ratio of 1:2:1 are mixed, dissolved in acetonitrile, refluxed at 90-150°C for 6-10 hours, and then water is added to quench the reaction. The organic phase is separated, the aqueous phase is extracted with an organic solvent, and the solvent is removed under reduced pressure to obtain a crude product. The crude product is purified by column chromatography to obtain a chiral ammonium salt of axial binaphthyl. Under the protection of inert gas, 9-boranebicyclo[3.3.1]nonane and a tetrahydrofuran solution of a chiral ammonium salt of axial binaphthyl are mixed, wherein the molar ratio of 9-boranebicyclo[3.3.1]nonane to the chiral ammonium salt of axial binaphthyl is 1:1, and then reacted at 40-60°C for 2-12 hours, filtered, and the filter cake is washed with n-hexane for multiple times, and vacuum dried to obtain a bifunctional catalyst 2.

[0024] In the class of chiral organoboron catalysts, the synthesis reaction equation of the main catalyst 1 of the two-component catalyst is:

[0025]

[0026] The specific preparation steps of the main catalyst 1 of the two-component catalyst are:

[0027] Under the protection of inert gas, (R)-spirocyclodiphenol, trifluoromethanesulfonic anhydride and pyridine in a molar ratio of 1:2:3 are mixed at 0°C, dissolved in dichloromethane, and then stirred at room temperature for 8 to 12 hours. After the reaction is completed, water is added to quench the reaction, the organic phase is separated, the aqueous phase is extracted with ethyl acetate, and the solvent is removed under reduced pressure to obtain a crude product. The crude product is purified by column chromatography to obtain a trifluoromethanesulfonate product. Under the protection of inert gas, tetrakis(triphenylphosphine)palladium, trifluoromethanesulfonate product and zinc cyanide in a molar ratio of 1:10:20 are mixed, dissolved in N,N-dimethylformamide, and then placed at 110 to 150°C for 12 to 24 hours. The reaction mixture is diluted with ethyl acetate, and washed with saturated sodium chloride solution and saturated sodium carbonate solution in turn, and the solvent is removed by rotary evaporation to obtain a crude product. The crude product is purified by column chromatography to obtain a cyano product. The cyanation product is mixed with an excess of acid and stirred at 130-160°C for 32-48 hours. The acid is a mixture of HOAc, H2O and H2SO4 in a volume ratio of 1:2:3. A small amount of water is added for dilution, extracted with ethyl acetate, and concentrated under reduced pressure. The crude product is purified by column chromatography to obtain the corresponding carboxylic acid product. Under the protection of inert gas, the carboxylic acid product and the tetrahydrofuran solution of lithium aluminum hydride are mixed, wherein the molar ratio of the carboxylic acid product to lithium aluminum hydride is 1:10, and refluxed at 80-100°C for 12-24 hours. After adding water to quench the reaction, dilute hydrochloric acid is added until there is no obvious precipitation in the solution, the organic phase is separated, and the corresponding hydroxyl product is obtained after concentration under reduced pressure. Under the protection of inert gas, the hydroxyl product and pyridinium chlorochromate (PCC) in a molar ratio of 1:3 are dissolved in dichloromethane and stirred at room temperature for 5-10 hours. Concentrated under reduced pressure, the reaction product is purified by column chromatography to obtain the corresponding aldehyde product. Under the protection of inert gas, the aldehyde product, methyl triphenylphosphine iodide (PPh3MeI), and potassium tert-butoxide in a molar ratio of 1:10:10 are mixed, dissolved in tetrahydrofuran, and reacted at room temperature for 5 to 12 hours. Water is added to quench the reaction, the organic phase is separated, and the crude product is obtained after reduced pressure concentration. The crude product is purified by column chromatography to obtain (R)-spirocyclodiene. Under the protection of inert gas, 9-boranebicyclo[3.3.1]nonane and (R)-spirocyclodiene tetrahydrofuran solution are mixed, wherein the molar ratio of 9-boranebicyclo[3.3.1]nonane to (R)-spirocyclodiene is 2:1, reacted at 40 to 60°C for 2 to 12 hours, filtered, the filter cake is washed with n-hexane for multiple times, and vacuum dried to obtain the main catalyst 1 of the two-component catalyst.

[0028] In the class of chiral organoboron catalysts, the synthesis reaction equation of the main catalyst 2 of the two-component catalyst is:

[0029]

[0030] The specific preparation steps of the main catalyst 2 of the two-component catalyst are:

[0031] Under the protection of inert gas, 9-borabicyclo[3.3.1]nonane and a tetrahydrofuran solution of (1S)-(-)-β-pinene are mixed, wherein the molar ratio of 9-borabicyclo[3.3.1]nonane to (1S)-(-)-β-pinene is 1:1, and reacted at 40-60° C. for 2-12 hours, and then filtered. The filter cake is washed with n-hexane for multiple times, and vacuum dried to obtain the main catalyst 2 of the two-component catalyst.

[0032] A method for preparing optically active polycarbonate or polyester using a chiral organoboron catalyst, the reaction equation is:

[0033]

[0034] The specific reaction process is: adding a chiral organoboron catalyst, meso-epoxy alkane and cyclic anhydride or carbon dioxide into a high-pressure reactor, adding an organic solvent, stirring until there is no obvious anhydride solid in the reaction liquid or the expected epoxy consumption is reached, and then stopping the reaction; first dissolving the crude product in dichloromethane, then adding methanol, and stirring vigorously to precipitate the polymer, and repeatedly repeating the precipitation process to obtain optically active polycarbonate or polyester.

[0035] The inert gas is nitrogen or argon.

[0036] The organic solvent is one or a mixture of two or more of tetrahydrofuran, toluene, dichloromethane, n-hexane and acetonitrile.

[0037] The cyclic anhydride:

[0038] for One or a mixture of two or more of the following;

[0039] The meso-alkylene oxide:

[0040] One or a mixture of two or more of the following;

[0041] The molar ratio of the meso-epoxy alkane to the chiral organic boron catalyst is 500:1 to 200000:1.

[0042] The molar ratio of the meso-epoxy alkane to the cyclic anhydride is 1:1 to 5:1.

[0043] When carbon dioxide is added, the carbon dioxide pressure is 0.1-5.0 MPa.

[0044] The reaction temperature is -20 to 150°C.

[0045] The reaction time is 0.1 to 80 hours.

[0046] The optically active polyester or polycarbonate has a molecular weight of 1000 to 1000000 g / mol and a molecular weight distribution of 1.05 to 2.50.

[0047] The content of carbonate units in the optically active polycarbonate is higher than 95%; the content of ester units in the optically active polyester is higher than 90%, and the enantioselectivity of carbonate units and ester units in the optically active polycarbonate or polyester is between 10% and 80%.

[0048] Beneficial effects of the present invention

[0049] (1) It still has high catalytic activity at low catalyst concentration.

[0050] (2) The catalyst can catalyze the reaction efficiently over a wide temperature range.

[0051] (3) The catalyst has high activity and high selectivity for the polymer product; the molecular weight is controllable and has a narrow distribution, the operating temperature range is wide, and the polymer structure can be adjusted.

[0052] (4) Polycarbonate and polyester have completely alternating structures, and the selectivity and structural selectivity of the polymerization products are both higher than 90%, and the enantiomeric excess of the diol obtained after degradation is between 10 and 80%.

[0053] (5) Unlike polymerization catalyzed by metal catalysts, which results in polymer coloration, the polycarbonates and polyesters obtained by polymerization catalyzed by chiral organic catalysts are colorless.

[0054] (6) Since there is no metal residue in the polymer, the application of polycarbonate and polyester in fields such as food packaging and medical materials will be greatly expanded. DETAILED DESCRIPTION

[0055] The technical solution of the present invention is further described below through examples.

[0056] Embodiment 1-2 is an embodiment of a method for preparing a dual-functional catalyst 1-2; Embodiment 3-4 is an embodiment of a method for preparing a main catalyst 1-2 of a dual-component catalyst.

[0057] Examples 5-8 are examples of preparing optically active polycarbonates using the chiral organoboron catalyst of the present invention; Examples 9-12 are examples of preparing optically active polyesters using the chiral organoboron catalyst of the present invention.

[0058] The names and numbers of the bifunctional catalyst 1-2, the main catalyst 1-2 of the two-component catalyst, the co-catalyst, the meso-epoxy alkane and the cyclic anhydride are shown in the following formula.

[0059]

[0060] Embodiment 1:

[0061] The synthesis reaction equation of bifunctional catalyst 1 is:

[0062]

[0063] The specific preparation steps of the bifunctional catalyst 1 are:

[0064] Under nitrogen protection, (R)-2,2'-bis(bromomethyl)-1,1'-binaphthyl (250 mg, 0.58 mmol), K2CO3 (160 mg, 1.16 mmol) and diallylamine (56 mg, 0.58 mmol) in a molar ratio of 1:2:1 were mixed, completely dissolved in acetonitrile, and then refluxed at 90°C for 10 h. Water was added to quench the reaction, and the organic phase was separated. The aqueous phase was extracted with dichloromethane (10 mL×3). The organic phases were combined and dried over anhydrous sodium sulfate. The solvent was removed by rotary evaporation. Finally, the crude product was purified by column chromatography to obtain the chiral ammonium salt of binaphthyl axial. Under nitrogen protection, the chiral ammonium salt of binaphthyl axial (0.3 g, 0.7 mmol) was dissolved in tetrahydrofuran, and then 9-boranebicyclo[3.3.1]nonane (2.8 mL) was slowly added dropwise. 0.5M tetrahydrofuran solution, 1.4 mmol), react at 60°C for 10 h. After concentration under reduced pressure, n-hexane was added, and a white solid precipitated at the bottom of the bottle, which was filtered, and the filter cake was washed with n-hexane (10 mL×3), and vacuum dried to obtain a bifunctional catalyst 1. 1 H NMR (600MHz, CDCl3): δ8.04–8.01(m,2H),7.98–7.97(m,2H),7.95–7.93(m,2H ),7.57–7.46(m,2H),7.36–7.35(m,3H),7.22–7.18(m,1H),5.09–4.98(m,2H) ,3.93–3.77(m,2H),3.62–3.60(m,2H),3.25–3.20(m,2H),1.88–1.65(m,12H) ,1.58–1.50(m,12H),1.38–1.35(m,4H),1.26–1.19(m,5H),1.11–1.03(m,3H).

[0065] Embodiment 2:

[0066] The synthesis reaction equation of bifunctional catalyst 2 is:

[0067]

[0068] The specific preparation steps of the bifunctional catalyst 1 are:

[0069] Under nitrogen protection, (R)-2,2'-bis(bromomethyl)-1,1'-binaphthyl (250 mg, 0.58 mmol), K2CO3 (160 mg, 1.16 mmol) and N-methylallylamine (41 mg, 0.58 mmol) in a molar ratio of 1:2:1 were mixed, completely dissolved in acetonitrile, and then refluxed at 90°C for 10 h, and then water was added to quench the reaction, and the organic phase was separated. The aqueous phase was extracted with dichloromethane (10 mL×3), the organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. Finally, the crude product was purified by column chromatography to obtain the chiral ammonium salt of binaphthyl axial; under nitrogen protection, the chiral ammonium salt of binaphthyl axial (0.3 g, 0.7 mmol) was dissolved in tetrahydrofuran, and then 9-boranebicyclo[3.3.1]nonane (1.4 mL) was slowly added dropwise. 0.5M tetrahydrofuran solution, 0.7 mmol), react at 60°C for 10 h. After concentration under reduced pressure, n-hexane was added, and a white solid precipitated at the bottom of the bottle, which was filtered, and the filter cake was washed with n-hexane (10 mL×3), and vacuum dried to obtain the bifunctional catalyst 2. 1 H NMR (600MHz, CDCl3): δ8.01–7.93(m,6H),7.49–7.25(m,6H),5.21–5.02(m,2H) ,3.89–3.53(m,3H),3.51–3.29(m,4H),1.68–1.51(m,13H),1.35–1.00(m,5H).

[0070] Embodiment 3:

[0071] The synthesis reaction equation of the main catalyst 1 of the two-component catalyst is:

[0072]

[0073] The specific preparation steps of the main catalyst 1 of the two-component catalyst are:

[0074] Under nitrogen protection, (R)-spirocyclodiphenol (2.0 g, 2.1 mmol) was dissolved in dichloromethane, and pyridine (2.8 mL) and trifluoromethanesulfonic anhydride (3.3 mL) were added at 0°C. Then stirred at room temperature for 12 h. After the reaction was completed, water was added to quench the reaction, and the pH value of the mixture was adjusted to 6-7 with dilute hydrochloric acid (1 M) and saturated sodium bicarbonate solution. The organic phase was separated, and the aqueous phase was extracted with ethyl acetate (30 mL × 3). The solvent was removed under reduced pressure to obtain a crude product. The crude product was purified by column chromatography to obtain a trifluoromethanesulfonate product. Under nitrogen protection, the trifluoromethanesulfonate product (5.0 g, 9.7 mmol), zinc cyanide (2.7 g, 22.5 mmol), and tetrakis(triphenylphosphine)palladium (1.2 g, 1.0 mmol) were dissolved in N,N-dimethylformamide, and then placed at 140°C for 24 h. The mixture was diluted with an appropriate amount of ethyl acetate, and washed with saturated sodium chloride solution and saturated sodium carbonate solution in turn. The solvent was removed by rotary evaporation to obtain a crude product, which was purified by column chromatography to obtain a cyanation product. The cyanation product (3.5 g, 13.0 mmol), H2O (60 mL), HOAc (30 mL) and H2SO4 (90 mL) were mixed and stirred at 145 ° C for 48 h. A small amount of water was added for dilution, and ethyl acetate (100 mL × 3) was used for extraction. The organic phases were combined and concentrated under reduced pressure. The crude product was purified by column chromatography to obtain the corresponding carboxylic acid product. Under nitrogen protection, lithium aluminum hydride (2.5 g, 64.9 mmol) was dissolved in tetrahydrofuran, and a tetrahydrofuran solution of the carboxylic acid product (2.0 g, 6.49 mmol) was added to the reaction system at 0 ° C, and the stirring was continued at 0 ° C for 30 min, and then the temperature was gradually raised to 80 ° C and refluxed for 24 h. Add water to quench the reaction, add dilute hydrochloric acid (1M) until there is no obvious precipitation in the solution, separate the organic phase, and concentrate under reduced pressure to obtain the corresponding hydroxyl product. Under nitrogen protection, the hydroxyl product (1.6g, 5.59mmol) and pyridinium chlorochromate (3.6g, 16.8mmol) were dissolved in dichloromethane and stirred at room temperature for 5h. After reduced pressure concentration, the crude product was purified by column chromatography to obtain the corresponding aldehyde product. Under nitrogen protection, methyltriphenylphosphonium iodide (7.5g, 18.5mmol) and potassium tert-butoxide (2.1g, 18.5mmol) were dissolved in tetrahydrofuran at 0℃, and the system was kept stirring at 0℃ for 30min. After adding the tetrahydrofuran solution of the aldehyde product (0.5g, 1.85mmol), the system can gradually return to room temperature and react at room temperature for 12h. Water was added to quench the reaction, the organic phase was separated, and the crude product was obtained after concentration under reduced pressure. The crude product was purified by column chromatography to obtain (R)-spirocyclodiene. Under nitrogen protection, (R)-spirocyclodiene (0.3 g, 1.1 mmol) was dissolved in tetrahydrofuran, and then 9-boranebicyclo[3.3.1]nonane (4.4 mL 0.5 M tetrahydrofuran solution, 2.2 mmol) was slowly added dropwise, and the reaction was carried out at 60°C for 10 h.After concentrating under reduced pressure, n-hexane was added, and a white solid precipitated out at the bottom of the bottle. The solid was filtered, and the filter cake was washed with n-hexane (10 mL×3) and dried in vacuo to obtain the main catalyst 1 of the two-component catalyst. 1 H NMR (400MHz, CDCl3): δ7.14–7.11(m,2H),7.05(d,J=8.0Hz,2H),7.00(d,J=8.0Hz,2H),3.09 –2.93(m,4H),2.42–2.15(m,8H),1.80–1.69(m,12H),1.57–1.40(m,16H),1.13–1.06(m,4H).

[0075] Embodiment 4:

[0076] The synthesis reaction equation of the main catalyst 2 of the two-component catalyst is:

[0077]

[0078] The specific preparation steps of the main catalyst 1 of the two-component catalyst are:

[0079] Under nitrogen protection, (1S)-(-)-β-pinene (0.5 g, 2.1 mmol) was dissolved in tetrahydrofuran, and then 9-borabicyclo[3.3.1]nonane (4.2 mL 0.5 M tetrahydrofuran solution, 2.1 mmol) was slowly added dropwise, and the mixture was reacted at 60°C for 10 h. After concentration under reduced pressure, n-hexane was added, and a white solid precipitated at the bottom of the bottle, which was filtered, and the filter cake was washed with n-hexane (10 mL × 3), and vacuum dried to obtain the main catalyst 2 of the two-component catalyst. 1 HNMR(600MHz, CDCl3): δ2.41–2.39(m,1H),2.05–2.01(m,1H),1.86–1.85(m,9H),1 .76–1.68(m,9H),1.48–1.40(m,2H),1.26–1.22(m,3H),1.20(s,3H),0.87(s,3H).

[0080] Example 5: A 20 mL autoclave equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. Under an argon atmosphere, a homogeneous solution of bifunctional catalyst 1 (R=H) and CHO at a molar ratio of 1:500 was injected into the autoclave, and 2.0 MPa of carbon dioxide was introduced after the autoclave was sealed. After reacting at 25°C for 24 hours, stirring was stopped and unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis showed that the conversion frequency was 14h -1, the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 6.0 Kg / mol and the molecular weight distribution is 1.20 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 20% by chiral gas chromatography.

[0081] Example 6: A 20 mL autoclave equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. Under an argon atmosphere, a homogeneous solution of bifunctional catalyst 1 (R = Ar) and CHO at a molar ratio of 1:500 was injected into the autoclave, and 2.0 MPa of carbon dioxide was introduced after the autoclave was sealed. After reacting at 25°C for 72 hours, stirring was stopped and unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis, the conversion frequency can be calculated to be 3h -1 , the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 6.8Kg / mol and the molecular weight distribution is 1.20 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 68% by chiral gas chromatography.

[0082] Example 7: A 20 mL autoclave equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. In an argon atmosphere, a homogeneous solution of a two-component catalyst consisting of the main catalyst 1, the cocatalyst PPNCl and CHO in a molar ratio of 1:1:500 was injected into the autoclave, and 2.0 MPa of carbon dioxide was introduced after the autoclave was sealed. After reacting at 25°C for 3 hours, stirring was stopped and unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis, the conversion frequency can be calculated to be 30h -1 , the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 4.5Kg / mol and the molecular weight distribution is 1.20 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 24% by chiral gas chromatography.

[0083] Comparative Example 7-1: A 20mL autoclave equipped with a magnet was dried at 120°C for more than 12h, evacuated and cooled to room temperature, and filled with argon for use. In an argon atmosphere, a homogeneous solution of a two-component catalyst consisting of the main catalyst 1, the co-catalyst PPNCl and CHO in a molar ratio of 1:1:1000 was injected into the autoclave. After the autoclave was sealed, 2.0MPa of carbon dioxide was introduced and the reaction was carried out at 150°C. The carbon dioxide pressure of the reaction system can be kept constant by adjusting the valve. After 20 minutes of reaction, stirring was stopped and the unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis showed that the conversion frequency was 1033h -1 , the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 6.7Kg / mol and the molecular weight distribution is 1.17 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 16% by chiral gas chromatography.

[0084] Comparative Example 7-2: A 20 mL autoclave equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. In an argon atmosphere, a homogeneous solution of a two-component catalyst consisting of the main catalyst 1, the co-catalyst PPNCl and CHO in a molar ratio of 1:1:500 was injected into the autoclave, and the autoclave was sealed and 2.0 MPa of carbon dioxide was introduced. The autoclave was placed at -20°C for reaction. After the reaction was completed for 42 hours, stirring was stopped and the unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis, the conversion frequency can be calculated to be 3h -1 , the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 6.1 Kg / mol and the molecular weight distribution is 1.19 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 26% by chiral gas chromatography.

[0085] Comparative Example 7-3: A 100mL autoclave equipped with a magnet was dried at 120°C for more than 12h, evacuated and cooled to room temperature, and filled with argon for use. Under an argon atmosphere, a homogeneous solution of a two-component catalyst consisting of the main catalyst 1, the co-catalyst PPNCl and CHO in a molar ratio of 1:1:100000 was placed in an autoclave, the autoclave was sealed, 2.0MPa of carbon dioxide was introduced, and the reaction was allowed to proceed at 100°C. The carbon dioxide pressure of the reaction system could be kept constant by adjusting the valve. After 10h of reaction, stirring was stopped and the unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for1 H NMR analysis showed that the conversion frequency was 833 h -1 , the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 56.2 Kg / mol and the molecular weight distribution is 1.22 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 10% by chiral gas chromatography.

[0086] Comparative Example 7-4: A 100mL autoclave equipped with a magnet was dried at 120°C for more than 12h, evacuated and cooled to room temperature, and filled with argon for use. In an argon atmosphere, a homogeneous solution of a two-component catalyst consisting of the main catalyst 1, the co-catalyst PPNCl and CHO in a molar ratio of 1:1:200000 was injected into the autoclave, and 5.0MPa of carbon dioxide was introduced after the autoclave was sealed. The reaction was allowed to react at 100°C. The carbon dioxide pressure of the reaction system could be kept constant by adjusting the valve. After 24h of reaction, stirring was stopped and the unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis showed that the conversion frequency was 770 h -1 , the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 89.1 Kg / mol and the molecular weight distribution is 1.30 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 10% by chiral gas chromatography.

[0087] Comparative Example 7-5: A 20 mL autoclave equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. In an argon atmosphere, a homogeneous solution of a two-component catalyst consisting of the main catalyst 1, the co-catalyst PPNCl and CPO in a molar ratio of 1:1:500 was injected into the autoclave, and 2.0 MPa of carbon dioxide was introduced after the autoclave was sealed. After reacting at 25°C for 72 hours, stirring was stopped and unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis, the conversion frequency can be calculated to be 3h -1 , the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 17.4Kg / mol and the molecular weight distribution is 1.18 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 12% by chiral gas chromatography.

[0088] Comparative Example 7-6: A 20 mL autoclave equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. In an argon atmosphere, a homogeneous solution of a two-component catalyst consisting of the main catalyst 1, the co-catalyst PPNCl and CDO in a molar ratio of 1:1:500 was injected into the autoclave, and 2.0 MPa of carbon dioxide was introduced after the autoclave was sealed. After reacting at 25°C for 12 hours, stirring was stopped and unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis, the conversion frequency can be calculated to be 3h -1 , the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 3.4Kg / mol and the molecular weight distribution is 1.18 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 16% by chiral gas chromatography.

[0089] Comparative Example 7-7: A 20 mL autoclave equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. In an argon atmosphere, a homogeneous solution of a two-component catalyst consisting of the main catalyst 1, the co-catalyst PPNCl and CBO in a molar ratio of 1:1:500 was injected into the autoclave, and 2.0 MPa of carbon dioxide was introduced after the autoclave was sealed. After reacting at 25°C for 32 hours, stirring was stopped and unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis, the conversion frequency can be calculated to be 12h -1 , the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 13.0 Kg / mol and the molecular weight distribution is 1.16 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 22% by chiral gas chromatography.

[0090] Comparative Example 7-8: A 20 mL autoclave equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. In an argon atmosphere, a homogeneous solution of a two-component catalyst consisting of the main catalyst 1, the cocatalyst PPNCl and the CEO in a molar ratio of 1:1:500 was injected into the autoclave, and 2.0 MPa of carbon dioxide was introduced after the autoclave was sealed. After reacting at 25°C for 18 hours, stirring was stopped and unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis, the conversion frequency can be calculated to be 4h -1, the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 3.4Kg / mol and the molecular weight distribution is 1.27 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 14% by chiral gas chromatography.

[0091] Example 8: A 20 mL autoclave equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. In an argon atmosphere, a homogeneous solution of a two-component catalyst, the main catalyst 2, the co-catalyst PPNCl and CHO, with a molar ratio of 1:1:500, was injected into the autoclave. The autoclave was sealed and 0.1 MPa of carbon dioxide was introduced. After reacting at 25°C for 72 hours, stirring was stopped and unreacted carbon dioxide was slowly released. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis, the conversion frequency can be calculated to be 3h -1 , the carbonate unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polycarbonate is 7.5Kg / mol and the molecular weight distribution is 1.17 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 11% by chiral gas chromatography.

[0092] Example 9: A 10 mL Schulink bottle equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. Under an argon atmosphere, a mixed solution of bifunctional catalyst 1 (R=H), PA and CHO in a molar ratio of 1:250:1000 was injected into the Schulink bottle, and 0.2 mL of tetrahydrofuran was added as a solvent. The reaction system was sealed and stirred at 50°C. After 40 hours, the reaction solution was clear and no obvious solid cyclic anhydride was found, and the reaction was stopped. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis, the conversion frequency can be calculated to be 4h -1 , the ester unit content is 90%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polyester is 7.1 Kg / mol and the molecular weight distribution is 1.23 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 16% by chiral gas chromatography.

[0093] Example 10: A 10 mL Schulink bottle equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. Under an argon atmosphere, a mixed solution of bifunctional catalyst 2 (R=H), PA and CHO in a molar ratio of 1:250:1000 was injected into the Schulink bottle, and 0.2 mL of tetrahydrofuran was added as a solvent. The reaction system was sealed and stirred at 50°C. After 24 hours, the reaction solution was clear and no obvious solid cyclic anhydride was present, and the reaction was stopped. A very small amount of the reaction mixture was taken out and used for 1 HNMR analysis showed that the conversion frequency was 4h -1 , the ester unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polyester is 4.0 Kg / mol and the molecular weight distribution is 1.21 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 22% by chiral gas chromatography.

[0094] Example 11: A 10 mL Schulink bottle equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. Under an argon atmosphere, a mixed solution of bifunctional catalyst 2 (R = Ar), PA and CHO in a molar ratio of 1:250:1000 was injected into the Schulink bottle, and 0.2 mL of tetrahydrofuran was added as a solvent. The reaction system was sealed and stirred at 50°C. After 24 hours, the reaction solution was clear and no obvious solid cyclic anhydride was found, and the reaction was stopped. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis showed that the conversion frequency was 3.6 h -1 , the ester unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polyester is 3.8Kg / mol and the molecular weight distribution is 1.15 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 78% by chiral gas chromatography.

[0095] Example 12: A 10 mL Schulink bottle equipped with a magnet was dried at 120°C for more than 12 hours, evacuated and cooled to room temperature, and filled with argon for use. Under an argon atmosphere, a mixed solution of a two-component catalyst consisting of the main catalyst 2, the co-catalyst PPNCl, PA and CHO in a molar ratio of 1:1:1000:1000 was injected into the Schulink bottle, and 0.5 mL of tetrahydrofuran was added as a solvent. The reaction system was sealed and stirred at 50°C. After 72 hours, the reaction solution was clear and no obvious solid cyclic anhydride was present, so the reaction was stopped. A very small amount of the reaction mixture was taken out and used for 1 H NMR analysis, the conversion frequency can be calculated to be 2h -1, the ester unit content is greater than 99%. The remaining polymer product is dissolved in dichloromethane / precipitated with methanol, and the above operation is repeated three times and washed, and dried under vacuum to constant weight. The molecular weight of the polyester is 8.5 Kg / mol and the molecular weight distribution is 1.22 by gel permeation chromatography. The polymer is hydrolyzed into diols with a dilute NaOH solution, and its enantioselectivity is 14% by chiral gas chromatography.

Claims

1. A chiral organoboron catalyst, characterized in that: The chiral organoboron catalyst includes an organoboron-onium salt bifunctional catalyst and a bicomponent catalyst composed of an organoboron and an onium salt; wherein the organoboron-onium salt bifunctional catalyst is a bifunctional catalyst formed by assembling an organoboron Lewis acid center and a Lewis base onium salt into an axially chiral binaphthyl skeleton; the bicomponent catalyst composed of an organoboron and an onium salt is a main catalyst formed by introducing an organoboron Lewis acid center into a chiral skeleton, and a cocatalyst The general structural formula of the organic boron-onium salt bifunctional catalyst and the organic boron and onium salt bicomponent catalyst is as follows: In the formula, the specific structure of the organic boron-onium salt bifunctional catalyst is: The specific structure of the main catalyst of the organic boron and onium salt two-component catalyst is: Cocatalyst for organic boron-onium salt two-component catalyst The salt is bis(triphenylphosphine)-imino chloride (PPNCl), and its specific structure is:

2. The chiral organoboron catalyst according to claim 1, characterized in that: The synthesis reaction equation of the bifunctional catalyst 1 is: The specific preparation steps of the bifunctional catalyst 1 are: Under the protection of inert gas, (R)-2,2'-bis(bromomethyl)-1,1'-binaphthyl, K2CO3 and diallylamine in a molar ratio of 1:2:1 are mixed, dissolved in acetonitrile, refluxed at 90-150°C for 6-10 hours, and then water is added to quench the reaction, the organic phase is separated, the aqueous phase is extracted with an organic solvent, and the solvent is removed under reduced pressure to obtain a crude product, and the crude product is purified by column chromatography to obtain a chiral ammonium salt of axial binaphthyl; under the protection of inert gas, 9-boranebicyclo[3.3.1]nonane and a tetrahydrofuran solution of a chiral ammonium salt of axial binaphthyl are mixed, wherein the molar ratio of 9-boranebicyclo[3.3.1]nonane to the chiral ammonium salt of axial binaphthyl is 2:1, and then reacted at 40-60°C for 2-12 hours, filtered, the filter cake is washed with n-hexane for multiple times, and vacuum dried to obtain a bifunctional catalyst 1; The synthesis reaction equation of the bifunctional catalyst 2 is: The specific preparation steps of bifunctional catalyst 2 are: Under the protection of inert gas, (R)-2,2'-bis(bromomethyl)-1,1'-binaphthyl, K2CO3 and N-methylallylamine in a molar ratio of 1:2:1 are mixed, dissolved in acetonitrile, refluxed at 90-150°C for 6-10 hours, water is added to quench the reaction, the organic phase is separated, the aqueous phase is extracted with an organic solvent, the solvent is removed under reduced pressure to obtain a crude product, and the crude product is purified by column chromatography to obtain a chiral ammonium salt of axial binaphthyl; under the protection of inert gas, 9-boranebicyclo[3.3.1]nonane and a tetrahydrofuran solution of a chiral ammonium salt of axial binaphthyl are mixed, wherein the molar ratio of 9-boranebicyclo[3.3.1]nonane to the chiral ammonium salt of axial binaphthyl is 1:1, and then reacted at 40-60°C for 2-12 hours, filtered, the filter cake is washed with n-hexane for multiple times, and vacuum dried to obtain a bifunctional catalyst 2; The synthesis reaction equation of the main catalyst 1 of the two-component catalyst is: The specific preparation steps of the main catalyst 1 of the two-component catalyst are: Under the protection of inert gas, (R)-spirodiphenol, trifluoromethanesulfonic anhydride and pyridine in a molar ratio of 1:2:3 are mixed at 0°C, dissolved in dichloromethane, and then stirred at room temperature for 8-12 hours; after the reaction is completed, water is added to quench the reaction, the organic phase is separated, the aqueous phase is extracted with ethyl acetate, and the solvent is removed under reduced pressure to obtain a crude product, and the crude product is purified by column chromatography to obtain a trifluoromethanesulfonate product; under the protection of inert gas, tetrakis(triphenylphosphine)palladium, trifluoromethanesulfonate product and zinc cyanide in a molar ratio of 1:10:20 are mixed, dissolved in N,N-dimethylformamide, and then placed at 110-150°C for 1 hour. 2 to 24 hours; dilute the reaction mixture with ethyl acetate, wash with saturated sodium chloride solution and saturated sodium carbonate solution in turn, remove the solvent by rotary evaporation to obtain a crude product, purify the crude product by column chromatography to obtain a cyanation product; mix the cyanation product with excess acid, and stir at 130 to 160° C. for 32 to 48 hours, wherein the acid is a mixture of HOAc, H2O and H2SO4 in a volume ratio of 1:2:3; dilute with water, extract with ethyl acetate, and concentrate under reduced pressure, purify the crude product by column chromatography to obtain the corresponding carboxylic acid product; under the protection of inert gas, mix the carboxylic acid product and a tetrahydrofuran solution of lithium aluminum hydride Mix, wherein the molar ratio of the carboxylic acid product and lithium aluminum hydride is 1:10, and reflux at 80-100°C for 12-24 hours; after adding water to quench the reaction, add dilute hydrochloric acid until there is no obvious precipitation in the solution, separate the organic phase, and concentrate under reduced pressure to obtain the corresponding hydroxyl product; under the protection of inert gas, dissolve the hydroxyl product and pyridinium chlorochromate in dichloromethane in a molar ratio of 1:3, and stir at room temperature for 5-10 hours; concentrate under reduced pressure, and purify the reaction product by column chromatography to obtain the corresponding aldehyde product; under the protection of inert gas, mix the aldehyde product, methyltriphenylphosphonium iodide, After mixing with potassium tert-butoxide, dissolving with tetrahydrofuran, reacting at room temperature for 5 to 12 hours; adding water to quench the reaction, separating the organic phase, concentrating under reduced pressure to obtain a crude product, purifying the crude product by column chromatography to obtain (R)-spirocyclodiene; under the protection of inert gas, mixing 9-boranebicyclo[3.3.1]nonane and tetrahydrofuran solution of (R)-spirocyclodiene, wherein the molar ratio of 9-boranebicyclo[3.3.1]nonane to (R)-spirocyclodiene is 2:1, reacting at 40 to 60° C. for 2 to 12 hours, filtering, washing the filter cake with n-hexane for multiple times, and vacuum drying to obtain the main catalyst 1 of the two-component catalyst; The synthesis reaction equation of the main catalyst 2 of the two-component catalyst is: The specific preparation steps of the main catalyst 2 of the two-component catalyst are: Under the protection of inert gas, 9-borabicyclo[3.3.1]nonane and a tetrahydrofuran solution of (1S)-(-)-β-pinene are mixed, wherein the molar ratio of 9-borabicyclo[3.3.1]nonane to (1S)-(-)-β-pinene is 1:1, and reacted at 40-60° C. for 2-12 hours, and then filtered. The filter cake is washed with n-hexane for multiple times, and vacuum dried to obtain the main catalyst 2 of the two-component catalyst.

3. A method for preparing optically active polycarbonate or polyester using a chiral organoboron catalyst as claimed in claim 1, characterized in that: The reaction equation is: The specific reaction process is: adding a chiral organoboron catalyst, meso-epoxy alkane and cyclic anhydride or carbon dioxide into a reaction kettle, adding an organic solvent, stirring until there is no obvious anhydride solid in the reaction liquid or the expected epoxy consumption is reached, and then stopping the reaction; first dissolving the crude product in dichloromethane, then adding methanol, and stirring vigorously to precipitate the polymer, and repeatedly repeating the precipitation process to obtain optically active polycarbonate or polyester.

4. The method for preparing optically active polycarbonate or polyester using a chiral organoboron catalyst according to claim 3, characterized in that: The inert gas is nitrogen or argon; The organic solvent is one or a mixture of two or more of tetrahydrofuran, toluene, dichloromethane, n-hexane and acetonitrile; The cyclic anhydride: for One or a mixture of two or more of the following; The meso-alkylene oxide: for One or a mixture of two or more.

5. The method for preparing optically active polycarbonate or polyester using a chiral organoboron catalyst according to claim 3 or 4, characterized in that: The molar ratio of the meso-epoxy alkane to the chiral organoboron catalyst is 500:1 to 200000:1; The molar ratio of the meso-epoxy alkane to the cyclic anhydride is 1:1 to 5:1; When carbon dioxide is added, the carbon dioxide pressure is 0.1-5.0 MPa.

6. The method for preparing optically active polycarbonate or polyester using a chiral organoboron catalyst according to claim 3 or 4, characterized in that: The reaction temperature is -20 to 150°C; The reaction time is 0.1 to 80 hours.

7. The method for preparing optically active polycarbonate or polyester using a chiral organic boron catalyst according to claim 5, characterized in that: The reaction temperature is -20 to 150°C; The reaction time is 0.1 to 80 hours.

8. The method for preparing optically active polycarbonate or polyester using a chiral organoboron catalyst according to claim 3, 4 or 7, characterized in that: The optically active polyester or polycarbonate has a molecular weight of 1000 to 1000000 g / mol and a molecular weight distribution of 1.05 to 2.

50.

9. The method for preparing optically active polycarbonate or polyester using a chiral organic boron catalyst according to claim 5, characterized in that: The optically active polyester or polycarbonate has a molecular weight of 1000 to 1000000 g / mol and a molecular weight distribution of 1.05 to 2.

50.

10. A method for preparing optically active polycarbonate or polyester using a chiral organoboron catalyst according to claim 3, 4, 7 or 9, characterized in that: The content of carbonate units in the optically active polycarbonate is higher than 95%; the content of ester units in the optically active polyester is higher than 90%, and the enantioselectivity of carbonate units and ester units in the optically active polycarbonate or polyester is between 10% and 80%.