A method for co-disposing printing and dyeing sludge in cement kiln

Through the cement kiln co-processing method, combined with sludge degradation agents, the problems of land occupation and secondary pollution in traditional printing and dyeing sludge treatment methods are solved, achieving efficient degradation of sludge and high-quality production of cement clinker, and improving treatment efficiency. and environmental safety.

CN116119953BActive Publication Date: 2024-10-22ZHEJIANG HONGSHI ENVIRONMENTAL PROTECTION SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310277793.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-21
Publication Date
2024-10-22
Estimated Expiration
2043-03-21

AI Technical Summary

Technical Problem

The traditional printing and dyeing sludge treatment method has problems such as large land occupation, high potential risk and secondary pollution. It is also difficult to effectively degrade the toxic and harmful substances in the sludge, affecting environmental safety and health.

Method used

The cement kiln co-processing method is used to degrade the printing and dyeing sludge through the sludge tank, add raw clinker for filtering and kneading, and then add cement raw material for calcination. The sludge degradation agent is used to improve the degradation effect and turn waste into treasure. Green treatment.

Benefits of technology

It can effectively reduce the volume of sludge, increase the amount of sludge degradation, prepare hydrated cement with high surface area and high compressive strength, simplify the process, reduce the operating cost of sewage treatment plants, and realize the high-value application of low-quality sludge.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116119953B_ABST
    Figure CN116119953B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of building materials, and specifically to a method for co-disposing printing and dyeing sludge in a cement kiln; biomass materials are transported to a two-stage shearing machine to be sheared into small sections, and then the printing and dyeing sludge is transported into a sludge pool by a screw conveyor, water is added to dilute the sludge pool, clinker powder is added, and after sufficient stirring, it is pumped to a plate and frame filter press to obtain a mud cake, and raw material powder is added to a double-screw mixer, and cement raw material is added after kneading, and it is entered into a rotary kiln as a raw material for the production of cement clinker for calcination. This method can realize the green treatment of printing and dyeing sludge by turning waste into treasure, and the prepared cooked cement has excellent compressive strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of printing and dyeing sludge treatment, in particular to a method for co-disposing printing and dyeing sludge with a cement kiln. Background Art

[0002] With the rapid development of industrial production and the continuous growth of urban population, especially with the continuous improvement of people's living standards, the total amount of industrial wastewater (especially textile printing and dyeing wastewater) and urban domestic wastewater is increasing day by day. According to relevant environmental protection laws and regulations, combined with the requirements of pollution reduction, these printing and dyeing wastewaters must be pre-treated to meet the requirements for entering the pipe, and then discharged after centralized treatment at the sewage treatment plant. However, while these sewages are being pre-treated and deeply purified at the sewage treatment plant, a large amount of sludge will be produced, resulting in the phenomenon of "sludge siege"; these sludges not only have high water content and large volume, but also concentrate various toxic and harmful substances. If they are not safely disposed of, they will not only directly affect the normal operation of the sewage treatment plant, but also cause secondary pollution to the surrounding environment.

[0003] For example, Chinese patent CN202210997778.9 proposes a method for preparing a dehydrating agent for dyeing and printing sludge and conditioning the dehydrating agent for dyeing and printing sludge. Pine biochar is prepared under certain conditions, and mixed particles are prepared with graphene oxide, magnesium chloride and aluminum oxide as raw materials; pine biochar and mixed particles are used as raw materials; acrylamide is added for grafting, and black powder is obtained by drying; then the black powder is mixed with spinel powder, ground and sieved to obtain a dehydrating agent for dyeing and printing sludge. The prepared dehydrating agent for dyeing and printing sludge is used to condition the dyeing and printing sludge to improve the dehydration performance of the sludge. The sludge dehydrating agent of the present invention can effectively improve the dehydration performance of the sludge, and the moisture content of the sludge filter cake is reduced to 73.59%-79.55%, and the sludge specific resistance is reduced by 34.25%-72.21%.

[0004] For example, Chinese patent CN202210832985.9 provides a method for treating difficult-to-degrade organic wastewater with a printing and dyeing sludge charcoal-based adsorbent, comprising: taking printing and dyeing sludge as raw material and sequentially performing drying treatment, crushing treatment, carbonization treatment, and screening treatment to obtain a printing and dyeing sludge charcoal-based adsorbent; then directly putting the printing and dyeing sludge charcoal-based adsorbent into the difficult-to-degrade organic wastewater, performing adsorption treatment at room temperature, and obtaining purified effluent after adsorption treatment; or filling the printing and dyeing sludge charcoal-based adsorbent as filter material in a filter column, and then passing the difficult-to-degrade organic wastewater into the filter column for adsorption treatment to obtain purified effluent after adsorption treatment; the present invention, in view of the particularity of the printing and dyeing sludge raw material, obtains a mesoporous printing and dyeing sludge charcoal-based adsorbent through carbonization treatment, which has good adsorption performance for pollutants in difficult-to-degrade organic wastewater, can reduce the operating cost of sewage treatment plants to achieve waste treatment, and at the same time realize low-cost and high-value application of low-quality sludge.

[0005] The annual output of dyeing sludge produced by water treatment can reach about 21 million tons of textile dyeing sludge. Dyeing sludge mainly contains various dyes, surface active agents, additives, polycyclic aromatic hydrocarbons (PAHs), persistent organic pollutants (POPs) and heavy metals. If not properly handled, it is easy to cause secondary pollution to groundwater and soil, toxic to other organisms, and affect environmental safety and health. Traditional methods of dyeing sludge treatment include land utilization, sanitary landfill, composting and heat treatment. Although low cost and simple operation are the advantages of land utilization and sanitary landfill, the occupation of large areas of land and the potential dangers of land and fluids are not conducive to the future planning and development of cities and towns, and also lead to a large amount of loss of available energy and secondary pollution. Summary of the invention

[0006] In order to solve at least one of the technical problems raised in the above-mentioned background technology, the present invention provides a method for co-disposing of printing and dyeing sludge in a cement kiln. The printing and dyeing sludge is degraded in a sludge pool, and raw and clinker are added to obtain material by filtration and kneading. Subsequently, cement raw material is added and calcined as a raw material for the production of cement clinker, thereby realizing green treatment of printing and dyeing sludge by turning waste into treasure.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] A method for co-disposing printing and dyeing sludge in a cement kiln, the specific steps are as follows:

[0009] Step 1: According to the mass percentage, 1-5 parts of biomass materials are conveyed to two-stage shearing machines and sheared into small segments of 70-90 cm and 5-15 cm respectively (a);

[0010] Step 2: 6-6.5 parts of printing and dyeing sludge are conveyed into a sludge pool by a screw conveyor, water is added to dilute the sludge pool, 10-20% of clinker powder is added, and after being fully stirred for 10-15 minutes, the sludge is pumped to a plate and frame filter press, and the filtration pressure is maintained. After the filtration time is 55-60 minutes, a mud cake (b) is obtained;

[0011] Step 3: feeding (b) into a twin-screw mixer, spraying 0.5-1 parts of raw material powder into the upper part of the mixer, and fully mixing the raw material powder and (b) to obtain material (c), and feeding (c) and (a) into a kneading machine for kneading for 20-30 minutes to obtain material (d);

[0012] Step 4: The material (d) is conveyed into the buffer bin by a high-angle belt, and the lower part of the buffer bin is conveyed into the top of the cement kiln decomposition furnace near the tertiary air duct (position A) through a shaftless reamer. The interface between position A and the reamer is locked with a three-stage air lock valve;

[0013] Step 5: The obtained material (d) is mixed into cement raw material at a ratio of 10%-15% by mass, and is fed into a rotary kiln as a raw material for producing cement clinker, and calcined at 1200-1400°C.

[0014] Preferably, the biomass materials in step 1 are straw, wood chips, branches, etc.

[0015] Preferably, in step 2, the water content of the sludge pool after dilution with water is 95-98%.

[0016] Preferably, the filtration pressure in step 2 is 12-24 kg / cm2.

[0017] Preferably, the moisture content of the mud cake in step 2 is 55-60%

[0018] Preferably, the stirring time in step 3 is 30 to 60 minutes.

[0019] Preferably, in step 4, 6 to 10 air cannons are added outside position A, and when the material (d) is burned at position A, the air cannons are operated 1 to 2 times for every 3 to 5 minutes of burning.

[0020] Furthermore, since the sludge contains a large amount of extracellular polymers, the high molecular substances produced by such microorganisms will affect the dehydration effect, resulting in a high water content in the sludge, thereby generating a large amount of flue gas. For this reason, a sludge degrading agent is added in a concentration of 0.1-0.6% by mass of the printing and dyeing sludge for treatment in step 2.

[0021] Preferably, the preparation method of the sludge degradation agent is as follows:

[0022] S1: adding 50-100 parts of crushed pecan shell particles (10-70 mesh) to 500-1000 parts of dichloromethane and 220-252 parts of acryloyl chloride according to weight parts, stirring at 50-70° C. for 12-15 hours, filtering, and obtaining pecan shells containing acryloyl cellulose;

[0023] S2: Add 10-20 parts of (ferrocenyl) hexanethiol, 0.5-2 parts of zinc maleate, 3-6 parts of sodium tert-butoxide, 100-200 parts of walnut shells of acryl cellulose, and 1000-1200 parts of dichloromethane according to mass proportions, react at controlled temperature, filter, and dry to obtain a sludge degrading agent.

[0024] Preferably, the reaction temperature in S2 is 50-70° C., and the reaction time is 100-150 min.

[0025] Reaction mechanism:

[0026] In the invention, (ferrocenyl) hexanethiol, zinc maleate, walnut shell of acryl cellulose undergoes a mercapto addition reaction to obtain a sludge degrading agent containing functional groups such as ferrocenyl and zinc carboxylate.

[0027] Beneficial effects:

[0028] 1. This method uses (ferrocenyl) hexanethiol, zinc maleate, and propylene cellulose to react with walnut shells to produce a thiol addition reaction to obtain a sludge degrading agent containing ferrocenyl, zinc carboxylate and other functional groups, which effectively increases the degradation of printing and dyeing sludge and is of great significance for sludge reduction.

[0029] 2. This method uses a cement kiln to co-dispose of printing and dyeing sludge, mixes it with cement raw material, and calcines it as a raw material for the production of cement clinker, thereby realizing green treatment of printing and dyeing sludge by turning waste into treasure.

[0030] 3. The cooked cement prepared by this method has a high specific surface area, high compressive strength and simple process. DETAILED DESCRIPTION

[0031] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0032] Example 1

[0033] A method for co-disposing printing and dyeing sludge in a cement kiln, the specific steps are as follows:

[0034] Step 1: 10 kg of biomass material is transported to two-stage shearing machines and cut into 70 cm and 5 cm small segments respectively (a);

[0035] Step 2: 60 kg of printing and dyeing sludge was conveyed into a sludge pool by a screw conveyor, water was added to dilute the sludge pool, 10% of clinker powder was added, and after being fully stirred for 10 minutes, it was pumped to a plate and frame filter press, and the filtration pressure was maintained. After 55 minutes of filtration time, a mud cake (b) was obtained;

[0036] Step 3: feeding (b) into a twin-screw mixer, spraying 5 kg of raw material powder into the upper part of the mixer, and fully mixing the raw material powder with (b) to obtain material (c), and feeding (c) and (a) into a kneading machine for kneading for 20 minutes to obtain material (d);

[0037] Step 4: The material (d) is conveyed into the buffer bin by a high-angle belt, and the lower part of the buffer bin is conveyed into the top of the cement kiln decomposition furnace near the tertiary air duct (position A) through a shaftless reamer. The interface between position A and the reamer is locked with a three-stage air lock valve;

[0038] Step 5: The obtained material (d) is mixed with cement raw material at a ratio of 10%, and the raw material is put into a rotary kiln as a raw material for producing cement clinker, and calcined at 1200°C.

[0039] The biomass materials in step 1 are straw, wood chips, branches, etc.

[0040] In the step 2, the water content of the sludge pool after dilution with water is 95%.

[0041] The filtration pressure in step 2 is 12 kg / cm2.

[0042] The moisture content of the mud cake in step 2 is 55%

[0043] The stirring time in step 3 is 30 minutes.

[0044] In step 4, 6 air cannons are added outside position A. When the material (d) is burned at position A, the air cannon is operated once for every 3 minutes of burning.

[0045] Since the sludge contains a large amount of extracellular polymers, the high molecular substances produced by this microorganism will affect the dehydration effect, resulting in a high water content in the sludge, thereby generating a large amount of flue gas. For this reason, 0.1% of the mass percentage of the printing and dyeing sludge is added in step 2 for treatment.

[0046] The preparation method of the sludge degradation agent is as follows:

[0047] S1: adding 50 g of crushed pecan shell particles (10-70 mesh) to 500 g of dichloromethane and 220 g of acryloyl chloride, stirring at 50° C. for 12 h, filtering, and obtaining pecan shells containing acryloyl cellulose;

[0048] S2: Add 10 g of (ferrocenyl) hexanethiol, 0.5 g of zinc maleate, 3 g of sodium tert-butoxide, 100 g of walnut shell of acrylcellulose, and 1000 g of dichloromethane, control the temperature to react, then filter and dry to obtain a sludge degrading agent.

[0049] The reaction temperature in S2 is 50° C. and the reaction time is 100 min.

[0050] Example 2

[0051] A method for co-disposing printing and dyeing sludge in a cement kiln, the specific steps are as follows:

[0052] Step 1: 30 kg of biomass materials are transported to two-stage shearing machines and cut into 80 cm and 10 cm small segments respectively (a);

[0053] Step 2: 65 kg of printing and dyeing sludge was conveyed into a sludge pool by a screw conveyor, water was added to dilute the sludge pool, 15% of clinker powder was added, and after being fully stirred for 12 minutes, it was pumped to a plate and frame filter press, and the filtration pressure was maintained. After 55 minutes of filtration time, a mud cake (b) was obtained;

[0054] Step 3: feeding (b) into a twin-screw mixer, spraying 7.5 kg of raw material powder into the upper part of the mixer, and fully mixing the raw material powder and (b) to obtain material (c), and feeding (c) and (a) into a kneading machine for kneading for 25 minutes to obtain material (d);

[0055] Step 4: The material (d) is conveyed into the buffer bin by a high-angle belt, and the lower part of the buffer bin is conveyed into the top of the cement kiln decomposition furnace near the tertiary air duct (position A) through a shaftless reamer. The interface between position A and the reamer is locked with a three-stage air lock valve;

[0056] Step 5: The obtained material (d) is mixed with cement raw material at a ratio of 12%, and is fed into a rotary kiln as a raw material for producing cement clinker and calcined at 1300°C.

[0057] The biomass materials in step 1 are straw, wood chips, branches, etc.

[0058] In step 2, the water content of the sludge pool after dilution with water is 96%.

[0059] The filtration pressure in step 2 is 18 kg / cm2.

[0060] The moisture content of the mud cake in step 2 is 60%

[0061] The stirring time in step 3 is 45 minutes.

[0062] In step 4, 8 air cannons are added outside position A. When the material (d) is burned at position A, the air cannon is operated once for every 4 minutes of burning.

[0063] Since the sludge contains a large amount of extracellular polymers, the high molecular substances produced by this microorganism will affect the dehydration effect, resulting in a high water content in the sludge, thereby generating a large amount of flue gas. For this reason, 0.3% of the mass percentage of the printing and dyeing sludge is added in step 2 for treatment.

[0064] The preparation method of the sludge degradation agent is as follows:

[0065] S1: adding 75 g of crushed pecan shell particles (10-70 mesh) to 750 g of dichloromethane and 234 g of acryloyl chloride, stirring at 60° C. for 14 h, filtering, and obtaining pecan shells containing acryloyl cellulose;

[0066] S2: Add 15 g of (ferrocenyl) hexanethiol, 1.3 g of zinc maleate, 4.5 g of sodium tert-butoxide, 150 g of walnut shell of acryl cellulose, and 1100 g of dichloromethane, control the temperature to react, then filter and dry to obtain a sludge degrading agent.

[0067] The reaction temperature in S2 is 60° C. and the reaction time is 125 min.

[0068] Example 3

[0069] A method for co-disposing printing and dyeing sludge in a cement kiln, the specific steps are as follows:

[0070] Step 1: 50 kg of biomass material is transported to two-stage shearing machines and cut into 90 cm and 15 cm small segments respectively (a);

[0071] Step 2: 65 kg of printing and dyeing sludge was conveyed into a sludge pool by a screw conveyor, water was added to dilute the sludge pool, 20% of clinker powder was added, and after being fully stirred for 15 minutes, it was pumped to a plate and frame filter press, and the filtration pressure was maintained. After 60 minutes of filtration time, a mud cake (b) was obtained;

[0072] Step 3: feeding (b) into a twin-screw mixer, spraying 10 kg of raw material powder into the upper part of the mixer, and fully mixing the raw material powder with (b) to obtain material (c), and feeding (c) and (a) into a kneading machine for kneading for 30 minutes to obtain material (d);

[0073] Step 4: The material (d) is conveyed into the buffer bin by a high-angle belt, and the lower part of the buffer bin is conveyed into the top of the cement kiln decomposition furnace near the tertiary air duct (position A) through a shaftless reamer. The interface between position A and the reamer is locked with a three-stage air lock valve;

[0074] Step 5: The obtained material (d) is mixed with cement raw material at a ratio of 15%, and is fed into a rotary kiln as a raw material for producing cement clinker and calcined at 1400°C.

[0075] The biomass materials in step 1 are straw, wood chips, branches, etc.

[0076] In step 2, the water content of the sludge pool after dilution with water is 98%.

[0077] The filtration pressure in step 2 is 24 kg / cm2.

[0078] The moisture content of the mud cake in step 2 is 60%

[0079] The stirring time in step 3 is 60 minutes.

[0080] In step 4, 10 air cannons are added outside position A. When the material (d) is burned at position A, the air cannons are operated twice for every 5 minutes of burning.

[0081] Since the sludge contains a large amount of extracellular polymers, the high molecular substances produced by this microorganism will affect the dehydration effect, resulting in a high water content in the sludge, thereby generating a large amount of flue gas. For this reason, 0.6% of the mass percentage of the printing and dyeing sludge is added in step 2 for treatment.

[0082] The preparation method of the sludge degradation agent is as follows:

[0083] S1: adding 100 g of crushed pecan shell particles (10-70 mesh) to 1000 g of dichloromethane and 252 g of acryloyl chloride, stirring at 70° C. for 15 h, filtering, and obtaining pecan shells containing acryloyl cellulose;

[0084] S2: Add 20 g of (ferrocenyl) hexanethiol, 2 g of zinc maleate, 6 g of sodium tert-butoxide, 200 g of walnut shell of acrylcellulose, and 1200 g of dichloromethane, control the temperature to react, then filter and dry to obtain a sludge degrading agent.

[0085] The reaction temperature in S2 is 70° C. and the reaction time is 150 min.

[0086] Comparative Example 1

[0087] A method for co-disposing printing and dyeing sludge in a cement kiln, the specific steps are as follows:

[0088] Step 1: 10 kg of biomass material is transported to two-stage shearing machines and cut into 70 cm and 5 cm small segments respectively (a);

[0089] Step 2: 60 kg of printing and dyeing sludge was conveyed into a sludge pool by a screw conveyor, water was added to dilute the sludge pool, 10% of clinker powder was added, and after being fully stirred for 10 minutes, it was pumped to a plate and frame filter press, and the filtration pressure was maintained. After 55 minutes of filtration time, a mud cake (b) was obtained;

[0090] Step 3: feeding (b) into a twin-screw mixer, spraying 5 kg of raw material powder into the upper part of the mixer, and fully mixing the raw material powder with (b) to obtain material (c), and feeding (c) and (a) into a kneading machine for kneading for 20 minutes to obtain material (d);

[0091] Step 4: The material (d) is conveyed into the buffer bin by a high-angle belt, and the lower part of the buffer bin is conveyed into the top of the cement kiln decomposition furnace near the tertiary air duct (position A) through a shaftless reamer. The interface between position A and the reamer is locked with a three-stage air lock valve;

[0092] Step 5: The obtained material (d) is mixed with cement raw material at a ratio of 10%, and is fed into a rotary kiln as a raw material for producing cement clinker and calcined at 1200°C.

[0093] The biomass materials in step 1 are straw, wood chips, branches, etc.

[0094] In the step 2, the water content of the sludge pool after dilution with water is 95%.

[0095] The filtration pressure in step 2 is 12 kg / cm2.

[0096] The moisture content of the mud cake in step 2 is 55%

[0097] The stirring time in step 3 is 30 minutes.

[0098] In step 4, 6 air cannons are added outside position A. When the material (d) is burned at position A, the air cannon is operated once for every 3 minutes of burning.

[0099] Comparative Example 2

[0100] A method for co-disposing printing and dyeing sludge in a cement kiln, the specific steps are as follows:

[0101] Step 1: 10 kg of biomass material is transported to two-stage shearing machines and cut into 70 cm and 5 cm small segments respectively (a);

[0102] Step 2: 60 kg of printing and dyeing sludge was conveyed into a sludge pool by a screw conveyor, water was added to dilute the sludge pool, 10% of clinker powder was added, and after being fully stirred for 10 minutes, it was pumped to a plate and frame filter press, and the filtration pressure was maintained. After 55 minutes of filtration time, a mud cake (b) was obtained;

[0103] Step 3: feeding (b) into a twin-screw mixer, spraying 5 kg of raw material powder into the upper part of the mixer, and fully mixing the raw material powder with (b) to obtain material (c), and feeding (c) and (a) into a kneading machine for kneading for 20 minutes to obtain material (d);

[0104] Step 4: The material (d) is conveyed into the buffer bin by a high-angle belt, and the lower part of the buffer bin is conveyed into the top of the cement kiln decomposition furnace near the tertiary air duct (position A) through a shaftless reamer. The interface between position A and the reamer is locked with a three-stage air lock valve;

[0105] Step 5: The obtained material (d) is mixed with cement raw material at a ratio of 10%, and is fed into a rotary kiln as a raw material for producing cement clinker and calcined at 1200°C.

[0106] The biomass materials in step 1 are straw, wood chips, branches, etc.

[0107] In the step 2, the water content of the sludge pool after dilution with water is 95%.

[0108] The filtration pressure in step 2 is 12 kg / cm2.

[0109] The moisture content of the mud cake in step 2 is 55%

[0110] The stirring time in step 3 is 30 minutes.

[0111] In step 4, 6 air cannons are added outside position A. When the material (d) is burned at position A, the air cannon is operated once for every 3 minutes of burning.

[0112] Since the sludge contains a large amount of extracellular polymers, the high molecular substances produced by this microorganism will affect the dehydration effect, resulting in a high water content in the sludge, thereby generating a large amount of flue gas. For this reason, 0.1% of the mass percentage of the printing and dyeing sludge is added in step 2 for treatment.

[0113] The preparation method of the sludge degradation agent is as follows:

[0114] S1: adding 50 g of crushed pecan shell particles (10-70 mesh) to 500 g of dichloromethane and 220 g of acryloyl chloride, stirring at 50° C. for 12 h, filtering, and obtaining pecan shells containing acryloyl cellulose;

[0115] S2: Add 0.5 g of zinc maleate, 3 g of sodium tert-butoxide, 100 g of cellulose-containing walnut shells, and 1000 g of dichloromethane, control the temperature to react, and then filter and dry to obtain a sludge degradation agent.

[0116] The reaction temperature in S2 is 50° C. and the reaction time is 100 min.

[0117] Comparative Example 3

[0118] A method for co-disposing printing and dyeing sludge in a cement kiln, the specific steps are as follows:

[0119] Step 1: 10 kg of biomass material is transported to two-stage shearing machines and cut into 70 cm and 5 cm small segments respectively (a);

[0120] Step 2: 60 kg of printing and dyeing sludge was conveyed into a sludge pool by a screw conveyor, water was added to dilute the sludge pool, 10% of clinker powder was added, and after being fully stirred for 10 minutes, it was pumped to a plate and frame filter press, and the filtration pressure was maintained. After 55 minutes of filtration time, a mud cake (b) was obtained;

[0121] Step 3: feeding (b) into a twin-screw mixer, spraying 5 kg of raw material powder into the upper part of the mixer, and fully mixing the raw material powder with (b) to obtain material (c), and feeding (c) and (a) into a kneading machine for kneading for 20 minutes to obtain material (d);

[0122] Step 4: The material (d) is conveyed into the buffer bin by a high-angle belt, and the lower part of the buffer bin is conveyed into the top of the cement kiln decomposition furnace near the tertiary air duct (position A) through a shaftless reamer. The interface between position A and the reamer is locked with a three-stage air lock valve;

[0123] Step 5: The obtained material (d) is mixed with cement raw material at a ratio of 10%, and is fed into a rotary kiln as a raw material for producing cement clinker and calcined at 1200°C.

[0124] The biomass materials in step 1 are straw, wood chips, branches, etc.

[0125] In the step 2, the water content of the sludge pool after dilution with water is 95%.

[0126] The filtration pressure in step 2 is 12 kg / cm2.

[0127] The moisture content of the mud cake in step 2 is 55%

[0128] The stirring time in step 3 is 30 minutes.

[0129] In step 4, 6 air cannons are added outside position A. When the material (d) is burned at position A, the air cannon is operated once for every 3 minutes of burning.

[0130] Since the sludge contains a large amount of extracellular polymers, the high molecular substances produced by this microorganism will affect the dehydration effect, resulting in a high water content in the sludge, thereby generating a large amount of flue gas. For this reason, 0.1% of the mass percentage of the printing and dyeing sludge is added in step 2 for treatment.

[0131] The preparation method of the sludge degradation agent is as follows:

[0132] S1: adding 50 g of crushed pecan shell particles (10-70 mesh) to 500 g of dichloromethane and 220 g of acryloyl chloride, stirring at 50° C. for 12 h, filtering, and obtaining pecan shells containing acryloyl cellulose;

[0133] S2: Add 10 g of (ferrocenyl) hexanethiol, 3 g of sodium tert-butoxide, 100 g of propylene cellulose in walnut shells, and 1000 g of dichloromethane, control the temperature to react, then filter and dry to obtain a sludge degrading agent.

[0134] The reaction temperature in S2 is 50° C. and the reaction time is 100 min.

[0135] The analysis of the printing and dyeing sludge content in the above examples and comparative examples is shown in the following table:

[0136]

[0137] The cooked cement prepared in the above examples and comparative examples was tested, and the results are shown in the following table:

[0138]

[0139]

[0140] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for co-processing printing and dyeing sludge in a cement kiln, comprising the following steps: Step 1: According to parts by mass, 1-5 parts of biomass material are transported to two shearing machines and cut to 70-90cm and 5-15cm, respectively, to obtain small segments (a); Step 2: 6 to 6.5 parts of printing and dyeing sludge were transported into the sludge pool by a screw conveyor, diluted with water in the sludge pool, 10 to 20% of clinker powder was added, stirred for 10 to 15 minutes, and then pumped to a plate and frame filter press, maintaining the filtration pressure, and the filtration time was 55 to 60 minutes to obtain a mud cake (b); Step 3: The mud cake (b) is fed into a twin-screw mixer, 0.5-1 parts of raw material powder is sprayed into the upper part of the mixer, the raw material powder and the mud cake (b) are fully stirred to obtain material (c), and the material (c) and the small segment (a) are fed into a kneader and kneaded for 20 to 30 minutes to obtain material (d); Step 4: Material (d) is conveyed into the buffer bin using a high-angle belt. The lower part of the buffer bin is fed into the top of the cement kiln decomposition furnace near the tertiary air duct through a shaftless reamer. The interface between the tertiary air duct and the reamer is locked with a three-stage air lock valve; Step 5: According to the mass fraction, the obtained material (d) is mixed with cement raw material in a ratio of 10%-15%, and the raw material for the production of cement clinker is entered into a rotary kiln and calcined at 1200-1400 ℃; Since the sludge contains a large amount of extracellular polymers, the high molecular weight substances produced by these microorganisms will affect the dehydration effect, resulting in a high water content in the sludge, thereby generating a large amount of flue gas. Therefore, in step 2, a sludge degrading agent is added at a concentration of 0.1-0.6% by mass of the printing and dyeing sludge for treatment; The preparation method of the sludge degradation agent is as follows: S1: According to the mass ratio, 50-100 parts of crushed pecan shell particles are added to 500-1000 parts of dichloromethane and 220-252 parts of acryloyl chloride, stirred at 50-70 ° C for 12-15h, filtered to obtain pecan shell containing propylene cellulose; S2: Add 10-20 parts of (ferrocenyl) hexanethiol, 0.5-2 parts of zinc maleate, 3-6 parts of sodium tert-butoxide, 100-200 parts of propylene cellulose walnut shells, and 1000-1200 parts of dichloromethane according to mass parts, control the temperature to react, then filter and dry to obtain a sludge degrading agent.

2. The method for co-processing printing and dyeing sludge in a cement kiln according to claim 1, characterized in that : The biomass materials in step 1 are straw, wood chips, and branches.

3. The method for co-processing printing and dyeing sludge in a cement kiln according to claim 1, characterized in that : In step 2, the water content of the sludge pool after dilution with water is 95-98%.

4. The method for co-processing printing and dyeing sludge in a cement kiln according to claim 1, characterized in that : The filter pressing pressure in step 2 is 12-24 kg / cm2.

5. The method for co-processing printing and dyeing sludge in a cement kiln according to claim 1, characterized in that : In step 2, the moisture content of the mud cake is 55-60%.

6. The method for co-processing printing and dyeing sludge in a cement kiln according to claim 1, characterized in that : The stirring time in step 3 is 30-60 minutes.

7. The method for co-processing printing and dyeing sludge in a cement kiln according to claim 1, characterized in that : In the step 4, 6-10 air cannons are added outside the tertiary air duct. When the material (d) is burned in the tertiary air duct, the air cannon is operated 1-2 times for every 3-5 minutes of burning.