Flame retardant polyamide material and preparation method and application thereof
By compounding aliphatic and aromatic polyamide resins in red phosphorus flame-retardant polyamide materials, and combining them with ethylene/zinc acrylate ion copolymer and glass fiber, the problem of insufficient oxygen index of traditional materials is solved and a high oxygen index is achieved. , good toughness and improved flame retardant properties, meeting the requirements of the EN45545 standard.
Patent Information
- Application Number
- CN202211683958.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-27
AI Technical Summary
The oxygen index of traditional red phosphorus flame-retardant polyamide materials cannot meet the risk level requirements in the EN45545 standard, and in the process of increasing the oxygen index, the toughness and wear resistance of the material will decrease.
Flame-retardant polyamide is formed by compounding aliphatic polyamide resin with aromatic polyamide resin formed by the condensation of m-xylylenediamine, and compatibility with ethylene/zinc acrylate ion copolymer and glass fiber with a certain degree of neutralization. The material uses the catalytic effect of ethylene/zinc acrylate ion copolymer and the carbon-forming effect of aromatic polyamide resin to improve the oxygen index and flame retardant properties of the material.
It significantly improves the oxygen index of the flame-retardant polyamide material, enhances its toughness and flame-retardant properties, meets the requirements of the HL3 risk level in the EN45545 standard, and broadens the application scenarios.
Smart Images

Figure CN116120740B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a flame retardant polyamide material and a preparation method and application thereof. Background Art
[0002] Polyamide, also known as nylon, is a heterochain polymer with an amide group in the main chain. Polyamide materials are used in the field of engineering plastics due to their excellent performance to replace some traditional metal materials. Due to the extensive use of polyamide materials in social production and life, the fire safety hazards inherent in polyamide materials have gradually attracted attention, and it is very necessary to modify them to be flame retardant.
[0003] There are many kinds of flame retardants for modifying polyamide. Phosphorus-based flame retardants have attracted widespread attention because they have flame retardant effects in both the condensed phase and the gas phase, and have outstanding performance in terms of smoke generation, corrosiveness and toxicity. Among them, red phosphorus forms a large amount of phosphoric acid substances during the combustion process, which can effectively promote the dehydration and carbonization of polymer materials and has outstanding flame retardant effects in the condensed phase. Red phosphorus flame retardant polyamide is widely used in electronic and electrical fields such as electrical switches, connectors and low-voltage circuit breakers due to its excellent flame retardant properties, mechanical properties, low smoke, high cost performance and electrical properties. An important application scenario in the field of electrical switches, connectors and low-voltage circuit breakers is the rail transit industry. The materials used in rail transit need to pass the EN45545 standard. The HL1 and HL2 risk levels in the EN45545 standard require the oxygen index of the material to be greater than or equal to 28%, and the HL3 risk level requires the oxygen index of the material to be greater than or equal to 32%. However, the oxygen index of traditional red phosphorus flame retardant polyamide can only reach about 26% to 27%, which cannot meet the risk level requirements in the EN45545 standard. Therefore, improving the oxygen index of red phosphorus flame retardant polyamide has very important technical theoretical significance and economic benefit significance.
[0004] There is a traditional technology that increases the oxygen index of red phosphorus flame retardant polyamide by adding melamine salt and organic modified nano-montmorillonite to red phosphorus flame retardant polyamide. Although the oxygen index can be increased to 29.2%, meeting the HL1 and HL2 risk level requirements of the EN45545 standard, the introduction of melamine salt will lead to poor thermal stability of the material and a narrower price window. At the same time, the introduction of organic modified nano-montmorillonite will cause a significant decrease in the toughness of the material. Therefore, the actual industrial application of this solution is of little significance.
[0005] There is also a traditional technology that compounds polyamide resin, red phosphorus flame retardant, polyphenylene sulfide resin, compatibilizer and synergist to prepare a red phosphorus flame retardant polyamide with high flame retardancy, and its oxygen index is only increased to 28%, which is limited. In addition, the compatibility of polyphenylene sulfide resin and polyamide resin is poor, resulting in reduced wear resistance and toughness of the flame retardant polyamide material.
[0006] In summary, there is currently no effective means to significantly improve the oxygen index of red phosphorus flame retardant polyamide. Although the traditional method of increasing the amount of red phosphorus added is helpful to improve the vertical combustion performance of the material, it has little effect on the oxygen index of the material. Summary of the invention
[0007] Based on this, the present invention provides a flame retardant polyamide material, which has a higher oxygen index and good toughness, flame retardant properties and strength.
[0008] The present invention is achieved through the following technical solutions.
[0009] A flame retardant polyamide material, comprising the following components, by weight: 25 to 90 parts of polyamide resin, 5 to 20 parts of red phosphorus flame retardant, 1 to 8 parts of ethylene / acrylic acid zinc ion copolymer and 20 to 50 parts of glass fiber;
[0010] Wherein, the polyamide resin includes aliphatic polyamide resin and aromatic polyamide resin;
[0011] The degree of neutralization of the ethylene / acrylic acid zinc ion copolymer by zinc ions is above 30%;
[0012] The aromatic polyamide resin is selected from one or more polymers prepared by polycondensation of monomers having the following structure:
[0013]
[0014] Wherein, n is 4, 6, 8 or 10;
[0015] The mass ratio of the aliphatic polyamide resin to the aromatic polyamide resin is (1-14):1.
[0016] In one embodiment, the composition includes the following components by weight: 40 to 65 parts of polyamide resin, 8 to 15 parts of red phosphorus flame retardant, 4 to 6 parts of ethylene / acrylic acid zinc ion copolymer and 25 to 35 parts of glass fiber.
[0017] In one embodiment, the neutralization degree of the ethylene / acrylic acid zinc ion copolymer by zinc ions is 30% to 90%.
[0018] In one of the embodiments, the mass ratio of the aliphatic polyamide resin to the aromatic polyamide resin is (2-5):1.
[0019] In one embodiment, the polyamide resin satisfies one or more of the following conditions:
[0020] (1) The aliphatic polyamide resin is selected from short-chain aliphatic polyamide resins; preferably, the aliphatic polyamide resin is selected from one or more of PA66, PA6 and PA56;
[0021] (2) The aromatic polyamide resin is selected from one or more of PA MXD6 and PA MXD10.
[0022] In one embodiment, the glass fiber is selected from one or more of E glass fiber, H glass fiber, S glass fiber, D glass fiber and C glass fiber.
[0023] In one embodiment, the red phosphorus flame retardant is a red phosphorus masterbatch; in the red phosphorus masterbatch, the mass percentage of red phosphorus is 40% to 60%.
[0024] In one embodiment, the limiting oxygen index of the flame retardant polyamide material is 32-39.
[0025] The present invention also provides a method for preparing the flame retardant polyamide material as described above, comprising the following steps:
[0026] mixing the components to prepare a premix;
[0027] The premix is melt-mixed and extruded into pellets.
[0028] The present invention also provides an application of the flame retardant polyamide material in the field of electronic appliances.
[0029] Compared with the prior art, the flame retardant polyamide material of the present invention has the following beneficial effects:
[0030] The invention prepares a flame retardant polyamide material having a high oxygen index, good flame retardancy, strength and toughness by compounding aliphatic polyamide resin and aromatic polyamide resin formed by condensation of meta-xylylenediamine to obtain a polyamide resin with good compatibility, and then compounding the polyamide resin with a red phosphorus flame retardant, an ethylene / acrylic acid zinc ion copolymer with a certain degree of neutralization and glass fiber in a certain mass ratio. Ethylene / acrylic acid zinc ion copolymer is a special elastomer coordinated by metal ions, which has good compatibility with polyamide. On the one hand, it has a toughening effect, which can make up for the poor toughness caused by the introduction of aromatic polyamide resin, and significantly improve the toughness of flame-retardant polyamide materials. On the other hand, the zinc ions in the ethylene / acrylic acid zinc ion copolymer with a certain degree of neutralization, as a transition metal, have a good catalytic carbonization effect, and compared with aliphatic polyamide, aromatic polyamide resin is easier to carbonize at high temperature; therefore, under the dual coupling of the catalytic effect of ethylene / acrylic acid zinc ion copolymer and the carbonization effect of aromatic polyamide resin formed by the condensation of meta-phenylenediamine, the flame-retardant polyamide quickly forms a dense carbon layer during the combustion process, which insulates heat and oxygen, thereby significantly improving the oxygen index of the flame-retardant polyamide material and broadening the application scenarios of the flame-retardant polyamide material. DETAILED DESCRIPTION
[0031] For ease of understanding of the present invention, the present invention will be described more fully below with reference to relevant embodiments. Preferred embodiments of the present invention are provided in the embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0032] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present invention, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.
[0033] In the present invention, when two or more "preferably" appear in one scheme, any two "preferably" may be independent of each other. The words "preferably", "more preferably" and the like in the present invention refer to embodiments of the present invention that may provide certain beneficial effects in certain cases. However, other embodiments may also be preferred under the same or other circumstances. In addition, the statement of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.
[0034] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0035] Unless otherwise specified, all percentages, fractions and ratios are calculated by the total mass of the composition of the present invention. Unless otherwise specified, all masses of the listed ingredients are given to the content of active substances, so they do not include solvents or by-products that may be contained in commercially available materials. The term "mass percentage content" herein can be represented by the symbol "%". Unless otherwise specified, all molecular weights in this article are weight average molecular weights expressed in Daltons. Unless otherwise specified, all formulations and tests in this article occur in an environment of 25°C. "Including", "including", "containing", "containing", "having" or other variants herein are intended to cover non-closed inclusions, and these terms are not distinguished. The term "comprising" means that other steps and ingredients that do not affect the final result can be added. The composition and method / process of the present invention include, consist of and are essentially composed of the necessary elements and restrictions described herein and any additional or optional ingredients, components, steps or restrictions described herein. The terms "efficacy", "performance", "effect" and "efficacy" are not distinguished between herein.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0037] The present invention provides a flame retardant polyamide material, which comprises the following components by weight: 25 to 90 parts of polyamide resin, 5 to 20 parts of red phosphorus flame retardant, 1 to 8 parts of ethylene / acrylic acid zinc ion copolymer and 20 to 50 parts of glass fiber;
[0038] Wherein, polyamide resin includes aliphatic polyamide resin and aromatic polyamide resin;
[0039] In the ethylene / acrylic acid zinc ion copolymer, the degree of neutralization by zinc ions is above 30%;
[0040] The aromatic polyamide resin is selected from one or more polymers prepared by polycondensation of monomers having the following structure:
[0041]
[0042] Wherein, n is 4, 6, 8 or 10;
[0043] The mass ratio of aliphatic polyamide resin to aromatic polyamide resin is (1-14):1.
[0044] Aromatic polyamide formed by condensation of meta-phenylenediamine can improve the flame retardant properties and oxygen index of flame retardant polyamide. Furthermore, aromatic polyamide formed by condensation of meta-phenylenediamine and ethylene / acrylic acid zinc ion copolymer have a good synergistic effect on improving the oxygen index of flame retardant polyamide materials: ethylene / acrylic acid zinc ion copolymer with a certain degree of neutralization can catalyze aromatic polyamide resin into carbon, covering the surface of flame retardant nylon, thereby insulating heat and oxygen, protecting the material from further erosion by flames, so there is a specific synergistic effect between ethylene / acrylic acid zinc ion copolymer and aromatic polyamide resin, specifically significantly improving the oxygen index of flame retardant polyamide. At the same time, using other similar copolymers to replace ethylene / acrylic acid zinc ion copolymer and aromatic polyamide resin compounding cannot obtain synergistic results. Similarly, using aromatic polyamide resin formed by condensation of other monomer structures and ethylene / acrylic acid zinc ion copolymer compounding cannot obtain synergistic results. In addition, the mass ratio of aliphatic polyamide resin to aromatic polyamide resin should be limited to the range of (1-14):1. If the mass ratio of aliphatic polyamide resin is too large, the oxygen index of flame retardant polyamide will also decrease.
[0045] Preferably, the flame retardant polyamide material comprises the following components, by weight: 40 to 65 parts of polyamide resin, 8 to 15 parts of red phosphorus flame retardant, 4 to 6 parts of ethylene / acrylic acid zinc ion copolymer and 25 to 35 parts of glass fiber.
[0046] It can be understood that in the present invention, the mass ratio of aliphatic polyamide resin to aromatic polyamide resin includes but is not limited to 1: 1, 2: 1, 3: 1, 4: 1, 5: 1, 6: 1, 7: 1, 8: 1, 9: 1, 10: 1, 11: 1, 12: 1, 13: 1, 14: 1. Preferably, the mass ratio of aliphatic polyamide resin to aromatic polyamide resin is (2-5): 1.
[0047] In another specific example, the flame retardant polyamide material includes the following components, measured in parts by weight: 20 to 70 parts of aliphatic polyamide resin, 5 to 20 parts of aromatic polyamide resin, 5 to 20 parts of red phosphorus flame retardant, 1 to 8 parts of ethylene / acrylic acid zinc ion copolymer and 20 to 50 parts of glass fiber.
[0048] Preferably, the flame retardant polyamide material comprises the following components, by weight: 30 to 50 parts of aliphatic polyamide resin, 10 to 15 parts of aromatic polyamide resin, 8 to 15 parts of red phosphorus flame retardant, 4 to 6 parts of ethylene / acrylic acid zinc ion copolymer and 25 to 35 parts of glass fiber.
[0049] In a specific example, the aliphatic polyamide resin is a short-chain aliphatic polyamide resin.
[0050] In a specific example, the aliphatic polyamide resin is selected from one or more of PA66, PA6 and PA56.
[0051] In a specific example, the aromatic polyamide resin is a semi-aromatic polyamide resin.
[0052] In a preferred example, n is 4 or 8.
[0053] In a specific example, the aromatic polyamide resin is selected from one or more of PA MXD6 and PA MXD10.
[0054] In a specific example, the neutralization degree of ethylene / acrylic acid zinc ion copolymer by zinc ion is 30% to 90%. Preferably, the neutralization degree of ethylene / acrylic acid zinc ion copolymer by zinc ion is 30% to 70%. Too much zinc ion content will also affect the carbonization of the material. Within the preferred range of 30% to 70% neutralization degree, the oxygen index of the flame retardant polyamide material can reach the HL3 risk level requirement in the EN45545 standard.
[0055] In a specific example, the content of acrylic acid in the ethylene / acrylic acid zinc ion copolymer is 8 wt% to 12 wt%. More specifically, the content of acrylic acid in the ethylene / acrylic acid zinc ion copolymer is 9 wt%.
[0056] In a specific example, the glass fiber is selected from one or more of E glass fiber, H glass fiber, S glass fiber, D glass fiber and C glass fiber.
[0057] Preferably, the glass fibers are selected from E glass fibers.
[0058] In a specific example, the red phosphorus flame retardant is a red phosphorus masterbatch; in the red phosphorus masterbatch, the mass percentage of red phosphorus is 40% to 60%.
[0059] More specifically, in the red phosphorus masterbatch, the mass percentage of red phosphorus is 50%.
[0060] In a specific example, the red phosphorus flame retardant is a microcapsule-encapsulated red phosphorus masterbatch.
[0061] In a specific example, the limiting oxygen index of the flame retardant polyamide material is 32 to 39. It can be understood that in the present invention, the limiting oxygen index of the flame retardant polyamide material includes but is not limited to 32, 33, 34, 35, 36, 37, 38 and 39.
[0062] The present invention also provides a method for preparing the flame retardant polyamide material, comprising the following steps:
[0063] Mixing the components to prepare a premix;
[0064] The premix is melt-mixed and extruded into pellets.
[0065] More specifically, the method for preparing the flame retardant polyamide material comprises the following steps:
[0066] Weigh each component by weight, put each component into a mixer and mix until uniform, to obtain a premix; then put the premix into a twin-screw extruder for melt mixing, and extrude granulation to obtain a high oxygen index red phosphorus flame retardant polyamide composite; wherein the twin-screw extruder has a screw aspect ratio of (40-48):1, a barrel temperature of 200°C-280°C, and a screw speed of 250rpm-350rpm.
[0067] The present invention also provides an application of the flame retardant polyamide material in the field of electronic appliances.
[0068] It can be understood that in the present invention, the field of electronic appliances includes but is not limited to electrical switches, connectors or low-voltage circuit breakers.
[0069] The flame retardant polyamide material and the preparation method thereof of the present invention are further described in detail below in conjunction with specific examples. The raw materials used in the following examples are all commercially available products unless otherwise specified.
[0070] PA66, grade PA66 EP-158, Huafeng Group;
[0071] PA6, brand PA6 HY-2800, Haiyang Chemical Fiber Company;
[0072] PA56, grade 1270W, Cathay Co., Ltd.;
[0073] PAMXD6 (n is 4), brand name AP-250, Yinggu Co., Ltd.;
[0074] PA MXD10 (n is 8), Yinggu Co., Ltd.;
[0075] PA66 / 6T, brand C1504T, Guangyin Co., Ltd.;
[0076] PA1010, brand TMFO F POL, Arkema Ltd.;
[0077] Glass fiber 1#, E glass fiber, brand ECS10-3.0-568H, China Jushi Co., Ltd.;
[0078] Glass fiber #2, S glass fiber, brand S-1HM435TM, Taishan Fiberglass Co., Ltd.;
[0079] Microcapsule coated red phosphorus flame retardant masterbatch, brand FR9950T, red phosphorus content 50%, Tongcheng Xinde Co., Ltd.
[0080] Ethylene / acrylic acid zinc ion copolymer #1, homemade, acrylic acid content 9%, of which 50% was neutralized by Zn particles;
[0081] Ethylene / acrylic acid zinc ion copolymer #2, homemade, acrylic acid content 9%, of which 70% is neutralized by Zn ions;
[0082] Ethylene / acrylic acid zinc ion copolymer #3, homemade, acrylic acid content 9%, of which 30% is neutralized by Zn ions;
[0083] Ethylene / acrylic acid zinc ion copolymer #4, homemade, acrylic acid content 9%, of which 90% is neutralized by Zn ions;
[0084] Ethylene / acrylic acid zinc ion copolymer #5, homemade, acrylic acid content 9%, of which 10% is neutralized by Zn ions;
[0085] Preparation method: LDPE, ZnO, Zn(CH3COO)2·2H2O, and Zn[CH3(CH2)16COO]2 were added to a Haake torque rheometer at 150°C and 50 r / min in appropriate proportions and kneaded for more than 10 minutes to prepare masterbatch 1. The temperature of the Haake torque rheometer was set to 190°C, and appropriate proportions of ethylene acrylic acid copolymer EAA (Escor5050, acrylic acid content 9wt%), masterbatch 1, and antioxidant 1010 were added to the Haake internal mixer in sequence for kneading. The reaction time was set to 6 minutes, and ethylene acrylic acid zinc ion copolymers with neutralization degrees of 10%, 30%, 50%, 70%, and 90% were prepared in sequence;
[0086] Maleic anhydride grafted modified POE, brand Fusabond N493, DuPont;
[0087] Ethylene methyl acrylate copolymer, brand Elvaloy AC resin 1125, DuPont.
[0088] According to the formula dosage (parts by weight) of specific embodiments 1 to 18 described in Tables 1 to 2 and comparative examples 1 to 11 described in Table 3, each component is weighed respectively, and each component is put into a mixer for mixing until uniform to obtain a premix; then the premix is put into a twin-screw extruder for melt mixing, and extruded and granulated to obtain a red phosphorus flame retardant polyamide composite; wherein the screw aspect ratio of the twin-screw extruder is (40 to 48): 1, the barrel temperature is 200° C. to 280° C., and the screw speed is 250 rpm to 350 rpm.
[0089] Effect verification test
[0090] The flame retardant polyamide materials prepared in the above Examples 1 to 18 and Comparative Examples 1 to 11 were subjected to effect verification experiments, including measuring flame retardancy, tensile properties, Izod notched impact strength and limiting oxygen index, as follows:
[0091] Flame retardant performance: The flame retardant performance of the sample strip is tested according to the relevant standards of UL 94, and the sample thickness is 0.8mm. Flame retardant performance is of great significance to electrical safety. The UL94 flame retardant grade needs to reach V-0 to meet application requirements.
[0092] Tensile properties: tested according to ISO 527-2 standard, tensile speed is 10mm / min;
[0093] Izod notched impact strength: tested according to ISO 178 standard, notch type is A;
[0094] Limiting Oxygen Index (LOI): According to ISO 4589-2:2017, the sample size is 125*10*4mm.
[0095] The formulations and effect verification experimental results of Examples 1 to 18 are shown in Tables 1 and 2.
[0096] Table 1
[0097]
[0098]
[0099] Table 2
[0100]
[0101]
[0102] The formulations and effect verification experimental results of Comparative Examples 1 to 11 are shown in Table 3.
[0103] Table 3
[0104]
[0105] According to the performance test results of the flame retardant polyamide materials prepared from Examples 1 to 18 in Table 1 and Table 2, the red phosphorus flame retardant polyamide material provided by the present invention has good strength, toughness, flame retardant properties and a high oxygen index. Specifically, the vertical combustion performance of the red phosphorus flame retardant polyamide material provided by the present invention can reach V-0, the oxygen index is 29.2% to 34.3%, the tensile strength is 118MPa to 172MPa, and the notched impact strength is 9.8kJ / m 2 ~15.2kJ / m 2 .
[0106] It can be seen from Example 3 and Comparative Example 2, Comparative Example 1 and Comparative Example 3 that the ethylene / acrylic acid zinc ion copolymer can not only improve the toughness of the red phosphorus halogen-free flame retardant polyamide composite, but also improve the oxygen index of the flame retardant polyamide material.
[0107] It can be seen from Example 3 and Comparative Example 3, and Comparative Example 1 and Comparative Example 2 that the aromatic polyamide resin can improve the tensile strength, flame retardant properties and oxygen index of the red phosphorus flame retardant polyamide composite, but has a certain effect on the toughness.
[0108] It can be seen from Example 3, Comparative Example 4 and Comparative Example 7 that although the use of conventional maleic anhydride grafted modified POE or ethylene butyl acrylate copolymer to replace ethylene / acrylic acid zinc ion copolymer can improve the toughness of halogen-free flame retardant polyamide, it will cause very serious damage to the flame retardant properties and oxygen index of red phosphorus flame retardant polyamide;
[0109] It can be seen from Example 3, Comparative Example 3 and Comparative Example 6 that the ethylene / acrylic acid zinc ion copolymer and the aromatic polyamide resin formed by the condensation of meta-phenylenediamine have a good synergistic effect to improve the oxygen index of the red phosphorus flame retardant polyamide. This is because the aromatic polyamide resin formed by the condensation of meta-phenylenediamine has a good carbonization effect, and the ethylene / acrylic acid zinc ion can catalyze the aromatic polyamide resin formed by the condensation of meta-phenylenediamine to form carbon, which covers the surface of the flame retardant nylon, thereby isolating heat and oxygen, and protecting the material from further erosion by the flame.
[0110] From Example 3, Comparative Example 5, Comparative Example 8 and Comparative Example 9, it can be seen that the zinc ion content in the ethylene / acrylic acid zinc ion copolymer will also affect the results. Too little content will lead to a decrease in the oxygen index, but it will help the tensile strength and toughness of the material to a certain extent, while adding too much will affect the carbonization of the material, resulting in a decrease in the oxygen index, and the tensile strength and toughness will deteriorate. At the same time, excessive acid will also catalyze the degradation of the material.
[0111] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0112] The above-described embodiments only express several implementation methods of the present invention, which are convenient for understanding the technical solutions of the present invention in detail, but they cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided by the present invention are all within the protection scope of the claims attached to the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the contents of the attached claims, and the description can be used to interpret the contents of the claims.
Claims
1. A flame retardant polyamide material, It is characterized in that The composition comprises the following components by weight: 25 to 90 parts of polyamide resin, 5 to 20 parts of red phosphorus flame retardant, 1 to 8 parts of ethylene / acrylic acid zinc ion copolymer and 20 to 50 parts of glass fiber; Wherein, the polyamide resin includes aliphatic polyamide resin and aromatic polyamide resin; The degree of neutralization of the ethylene / acrylic acid zinc ion copolymer by zinc ions is 30% to 70%; The aromatic polyamide resin is selected from one or more polymers prepared by polycondensation of monomers having the following structure: ; Wherein, n is 4, 6, 8 or 10; The mass ratio of the aliphatic polyamide resin to the aromatic polyamide resin is (1-14):
1.
2. The flame retardant polyamide material according to claim 1, It is characterized in that The invention comprises the following components in parts by weight: 40 to 65 parts of polyamide resin, 8 to 15 parts of red phosphorus flame retardant, 4 to 6 parts of ethylene / acrylic acid zinc ion copolymer and 25 to 35 parts of glass fiber.
3. The flame retardant polyamide material according to claim 1, It is characterized in that The mass ratio of the aliphatic polyamide resin to the aromatic polyamide resin is (2-5):
1.
4. The flame retardant polyamide material according to claim 1, It is characterized in that The polyamide resin satisfies one or more of the following conditions: (1) The aliphatic polyamide resin is selected from one or more of PA66, PA6 and PA56; (2) The aromatic polyamide resin is selected from one or more of PA MXD6 and PA MXD10.
5. The flame retardant polyamide material according to any one of claims 1 to 4, It is characterized in that The glass fiber is selected from one or more of E glass fiber, H glass fiber, S glass fiber, D glass fiber and C glass fiber.
6. The flame retardant polyamide material according to any one of claims 1 to 4, It is characterized in that The red phosphorus flame retardant is a red phosphorus masterbatch; in the red phosphorus masterbatch, the mass percentage of red phosphorus is 40% to 60%.
7. The flame retardant polyamide material according to any one of claims 1 to 4, It is characterized in that The limiting oxygen index of the flame retardant polyamide material is 32-39.
8. A method for preparing the flame retardant polyamide material according to any one of claims 1 to 7, It is characterized in that The steps include: mixing the components to prepare a premix; The premix is melt-mixed and extruded into pellets.
9. Use of the flame retardant polyamide material according to any one of claims 1 to 7 in the field of electronic appliances.
Citation Information
Patent Citations
Glow wire resistant polyamides
CN105121552A
Red phosphorus flame-retardant polyamide composite material as well as preparation method and application thereof
CN114395248A
Halogen-free flame-retardant polyamide composition with good toughness as well as preparation and application thereof
CN115449217A