Composite cathode and its coupling method for electrochemical oxidation reaction and catalytic hydrogenation reduction reaction
By coupling electrochemical oxidation and catalytic hydrogenation reduction reactions with a composite cathode and storing reduced hydrogen using a hydrogen storage alloy, the problem of low energy utilization efficiency in traditional electrochemical synthesis systems is solved, and a highly efficient organic synthesis process is achieved.
Patent Information
- Application Number
- CN202211694869.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-12-28
AI Technical Summary
Traditional electrochemical synthesis systems have low energy utilization efficiency and require stringent pairwise electrochemical synthesis conditions, making them difficult to apply in practical organic synthesis.
A composite cathode is employed, comprising a current collector and a coating. The coating material includes a hydrogen storage alloy, a conductive agent, and a binder, which is used to couple the electrochemical oxidation reaction with the catalytic hydrogenation reduction reaction. The hydrogen storage alloy stores reduced hydrogen and enables catalytic hydrogenation reduction without the need for an additional hydrogen source.
It improves the atom economy and energy utilization efficiency of electrochemical synthesis reaction systems, avoids high-energy-consuming product separation processes, and is suitable for the coupling design of various redox reactions.
Smart Images

Figure HDA0004022991230000011 
Figure HDA0004022991230000012 
Figure HDA0004022991230000021
Abstract
Description
Technical Field
[0001] This invention relates to the field of organic electrochemical preparation technology, and in particular to a composite cathode and a coupling method for its electrochemical oxidation reaction and catalytic hydrogenation reduction reaction. Background Technology
[0002] Electrochemical synthesis technology uses renewable electrical energy to drive redox reactions, replacing the oxidants or reducing agents required in traditional organic synthesis. It can also prepare target products under milder conditions, improving the atom economy, sustainability, and safety of the production process. In line with the current concept of sustainable development, it is an emerging green synthesis method that has attracted widespread attention from researchers and industry professionals in the field of organic synthesis.
[0003] Traditional electrochemical synthesis systems typically achieve high-value substrate conversion only on one electrode side, with side reactions involving solvents, electrolytes, or sacrificial electrodes occurring on the counter electrode side to achieve charge-mass balance. This results in low energy efficiency. The oxidation of alcohols to aldehydes, ketones, and carboxylic acids is one of the most important and widely used oxidation reactions in organic synthesis. However, hydrogen evolution occurs on the counter electrode side of traditional alcohol electrooxidation reactions, and separating and purifying the hydrogen obtained from the cathode for reuse is an energy-intensive process. Although paired electrochemical synthesis can improve energy efficiency through the coupling of reactions at the anode and cathode, the matching of parameters such as substrate, potential, and electrolyte at the two electrodes is demanding, making it difficult to obtain high-value paired systems. Therefore, the low energy efficiency of traditional electrochemical synthesis systems and the stringent coupling conditions of existing paired methods limit their practical application in organic synthesis. Summary of the Invention
[0004] Therefore, it is necessary to provide a composite cathode and its coupling method for electrochemical oxidation reaction and catalytic hydrogenation reduction reaction to address the above problems. The composite cathode can be used to couple electrochemical oxidation-catalytic hydrogenation reduction reactions under various reaction substrate conditions. The reaction system is simple, has wider applicability, and has high energy utilization efficiency for electrochemically synthesized materials.
[0005] A composite cathode includes a current collector and a coating disposed on the current collector. The coating material includes a hydrogen storage alloy material, a conductive agent, and a binder, wherein the hydrogen storage alloy material has a loading of 40 mg / cm² on the current collector. 2 -80mg / cm 2 ;
[0006] The activated composite cathode can be used as a cathode for electrochemical oxidation reactions. After electrochemical oxidation, the reduced composite cathode can be used for catalytic hydrogenation reduction reactions after rinsing. After catalytic hydrogenation reduction reactions, the composite cathode can be reactivated.
[0007] In one embodiment, the hydrogen storage alloy material is selected from AB5 type hydrogen storage alloy material, AB2 type hydrogen storage alloy material, AB type hydrogen storage alloy material or A2B type hydrogen storage alloy material.
[0008] In one embodiment, the conductive agent is selected from at least one of carbon black, copper powder, and nickel powder, and the mass ratio of the conductive agent to the hydrogen storage alloy material is 1:10-1:100.
[0009] And / or, the binder is selected from at least one of polytetrafluoroethylene, water-soluble rubber, and cellulose, and the mass ratio of the binder to the hydrogen storage alloy material is 1:10 to 1:100.
[0010] In one embodiment, the coating material further includes a catalyst selected from at least one of noble metals, metal oxides, and metal sulfides, wherein the mass ratio of the catalyst to the hydrogen storage alloy material is less than or equal to 1:100.
[0011] A method for coupling an electrochemical oxidation reaction with a catalytic hydrogenation reduction reaction includes the following steps:
[0012] Organic alcohol, electrolyte and first reaction solvent are mixed to form the first reaction substrate, which is added to the electrolytic cell. After the composite cathode is activated, it is placed in the electrolytic cell together with the anode. Electrochemical oxidation reaction is carried out by passing electricity to obtain aldehyde, ketone or acid.
[0013] After the electrochemical oxidation reaction is completed, the composite cathode is removed from the electrolytic cell and rinsed to obtain a reducing composite cathode;
[0014] Unsaturated organic compounds are mixed with a second reaction solvent to form a second reaction substrate, which is then added to an organic reaction tank and placed in the reducing composite cathode for catalytic hydrogenation reduction to obtain hydrogenated organic compounds.
[0015] After the catalytic hydrogenation reduction reaction is completed, a composite cathode is obtained.
[0016] In one embodiment, the activation method of the composite cathode includes: performing a constant current charge-discharge cycle experiment on the composite cathode in a potassium hydroxide solution.
[0017] In one embodiment, the organic alcohol is selected from at least one of fatty alcohols, alicyclic alcohols, and aromatic alcohols;
[0018] And / or, the first reaction solvent is selected from at least one of water, methanol, ethanol, acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran, and tert-butanol.
[0019] In one embodiment, the concentration of the organic alcohol in the first reaction substrate is 0.025 mol / L to 0.3 mol / L.
[0020] In one embodiment, the unsaturated organic compound is selected from at least one of alkyne-based organic compounds, olefin-based organic compounds, and nitro-based organic compounds;
[0021] And / or, the second reaction solvent is selected from at least one of water, methanol, ethanol, acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran, and tert-butanol.
[0022] In one embodiment, the concentration of the unsaturated organic compound in the second reaction substrate is 0.02 mol / L to 1 mol / L.
[0023] This invention utilizes a composite cathode to electrochemically reduce and store the reduced hydrogen required for subsequent reactions, while simultaneously enhancing its own activation activity. This replaces the traditional cathode hydrogen evolution reaction. By coupling a hydrogenation reduction reaction, the reduced hydrogen stored in the composite cathode itself serves as the reducing force, enabling catalytic hydrogenation reduction without an additional hydrogen source. This results in a highly atom-economical electrochemical synthesis reaction system with minimal waste and low energy consumption, thus improving the material and energy utilization efficiency of the reaction system. In the coupling process of the electrochemical oxidation and catalytic hydrogenation reduction reactions, simply moving the composite cathode between the alcohol electrochemical oxidation reactor and the hydrogenation catalytic reactor allows for the separate production of different high-value-added products in different reactors. This avoids the high-energy-consuming separation process required after different products are prepared at the two electrodes in an electrochemical oxidation-reduction reaction. Furthermore, it can couple electrochemical oxidation-catalytic hydrogenation reduction reactions with various reaction substrates, making it more flexible for coupling designs of multiple oxidation-reduction reactions and improving the material and energy utilization efficiency of the reaction system. Attached Figure Description
[0024] Figure 1 This is a flowchart illustrating the coupling method of electrochemical oxidation reaction and catalytic hydrogenation reduction reaction in one embodiment of the present invention.
[0025] Figure 2 This is a graph showing the change in discharge capacity of the composite cathode in Example 1 of the present invention during the activation process with the number of charge-discharge cycles;
[0026] Figure 3 This is a scanning electron microscope image of the surface coating of the composite cathode before reaction in Example 6 of this invention;
[0027] Figure 4 This is a scanning electron microscope image of the surface coating of the composite cathode in Example 6 of the present invention after five coupling experiment cycles. Detailed Implementation
[0028] To facilitate understanding of the present invention, it will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. Rather, these embodiments or examples are provided to make the disclosure of the present invention more thorough and complete.
[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments or examples only and is not intended to be limiting of the invention.
[0030] This invention provides a composite cathode, comprising a current collector and a coating disposed on the current collector. The coating material includes a hydrogen storage alloy material, a conductive agent, and a binder, wherein the hydrogen storage alloy material has a loading of 40 mg / cm² on the current collector. 2 -80mg / cm 2 ;
[0031] The activated composite cathode can be used as a cathode for electrochemical oxidation reactions. After electrochemical oxidation, the reduced composite cathode can be used for catalytic hydrogenation reduction reactions after rinsing. After catalytic hydrogenation reduction reactions, the composite cathode can be reactivated.
[0032] This invention utilizes a composite cathode to electrochemically reduce and store the reduced hydrogen required for subsequent reactions, while simultaneously enhancing its own activation activity. This replaces the traditional cathode hydrogen evolution reaction. By coupling a hydrogenation reduction reaction, the reduced hydrogen stored in the composite cathode itself serves as the reducing force, enabling catalytic hydrogenation reduction without an additional hydrogen source. This results in a highly atom-economical electrochemical synthesis reaction system with minimal waste and low energy consumption, thus improving the material and energy utilization efficiency of the reaction system. In the coupling process of the electrochemical oxidation and catalytic hydrogenation reduction reactions, simply moving the composite cathode between the alcohol electrochemical oxidation reactor and the hydrogenation catalytic reactor allows for the separate production of different high-value-added products in different reactors. This avoids the high-energy-consuming separation process required after different products are prepared at the two electrodes in an electrochemical oxidation-reduction reaction. Furthermore, it can couple electrochemical oxidation-catalytic hydrogenation reduction reactions with various reaction substrates, making it more flexible for coupling designs of multiple oxidation-reduction reactions and improving the material and energy utilization efficiency of the reaction system.
[0033] Specifically, the hydrogen storage alloy material is selected from AB5 type hydrogen storage alloy material, AB2 type hydrogen storage alloy material, AB type hydrogen storage alloy material or A2B type hydrogen storage alloy material.
[0034] A and B are each independently selected from transition metal elements.
[0035] Furthermore, the AB5-type hydrogen storage alloy material is preferably an AB5-type rare earth alloy with a hexagonal or orthorhombic crystal structure, more preferably LaNi5 or MmNi. a Mn b Al c Co d Wherein, a = 3.5-4.2, b = 0.2-0.7, c = 0.2-0.6, d = 0-0.7, a+b+c+d = 5, and Mm is a mixed rare earth element with lanthanum as the main element; the AB2 type hydrogen storage alloy material is preferably an AB2 type hydrogen storage alloy material with a Laves phase structure, more preferably ZnMn2; the AB type hydrogen storage alloy material is preferably an AB type alloy with a CsCl structure, further preferably a titanium alloy, more preferably TiFe or TiNi; the A2B type hydrogen storage alloy material is preferably a titanium alloy or a magnesium alloy, wherein the titanium alloy is more preferably Ti2Ni, and the magnesium alloy is more preferably Mg2Ni.
[0036] Optionally, the conductive agent is selected from at least one of carbon black, copper powder, and nickel powder, and the mass ratio of the conductive agent to the hydrogen storage alloy material is 1:10 to 1:100.
[0037] Optionally, the binder is selected from at least one of polytetrafluoroethylene (PTFE), water-soluble rubber, and cellulose, and the mass ratio of the binder to the hydrogen storage alloy material is 1:10 to 1:100.
[0038] Optionally, the current collector is selected from carbon materials, metallic materials, or conductive glass.
[0039] To further improve the catalytic performance of the composite cathode, the coating material also includes a catalyst, wherein the mass ratio of the catalyst to the hydrogen storage alloy material is less than or equal to 1:100.
[0040] Specifically, the catalyst is selected from at least one of noble metals, metal oxides, and metal sulfides.
[0041] It should be noted that in practical applications, the effective content of precious metals in precious metal catalysts is relatively low. Therefore, the mass ratio of precious metal catalyst to hydrogen storage alloy material refers to the mass ratio of the effective content of precious metals in the precious metal catalyst to the mass ratio of hydrogen storage alloy material.
[0042] In one embodiment, the method for preparing the composite cathode includes: mixing 100 parts by weight of hydrogen storage alloy material, 1-10 parts by weight of conductive agent, 1-10 parts by weight of binder, and 0-1 parts by weight of catalyst to prepare a slurry with a certain viscosity; coating the slurry onto the surface of a current collector; and then drying it at a constant temperature of 150℃-200℃ for 2 hours under a vacuum atmosphere to allow the coating to have good dispersion and adhesion under the action of the binder, thereby obtaining the composite cathode.
[0043] In one embodiment, the activation method of the composite cathode includes: performing a constant current charge-discharge cycle experiment on the composite cathode in a potassium hydroxide solution, wherein the concentration of the potassium hydroxide solution is 1 mol / L-8 mol / L; during the charge-discharge cycle, the charge-discharge rate is 0.1C-10C, and the number of cycles is 2-20.
[0044] Combination Figure 1 The method for coupling an electrochemical oxidation reaction with a catalytic hydrogenation reduction reaction provided by the present invention includes the following steps:
[0045] S1, organic alcohol, electrolyte and first reaction solvent are mixed to form the first reaction substrate and added to the electrolytic cell. After the composite cathode is activated, it is placed in the electrolytic cell together with the anode. Electrochemical oxidation reaction is carried out by passing electricity to obtain aldehyde, ketone or acid.
[0046] S2. After the electrochemical oxidation reaction is completed, the composite cathode is removed from the electrolytic cell and rinsed to obtain a reducing composite cathode.
[0047] S3, unsaturated organic matter is mixed with a second reaction solvent to form a second reaction substrate, which is added to an organic reaction tank and placed in the reducing composite cathode for catalytic hydrogenation reduction reaction to obtain hydrogenated organic matter;
[0048] After the catalytic hydrogenation reduction reaction S4 is completed, a composite cathode is obtained.
[0049] Unlike traditional electrochemical hydrogen evolution reactions, in step S1, an oxidation reaction occurs at the anode, converting the hydroxyl groups in the organic alcohol into aldehyde or carboxyl groups. Activation can activate the hydrogen storage function of the composite cathode, giving the activated composite cathode an excellent reduced hydrogen storage capacity during the electrochemical oxidation reaction. This allows the reduced hydrogen generated during the electrochemical oxidation process to be stored in the hydrogen storage alloy material in the coating without any hydrogen evolution side reactions, thus improving the energy utilization efficiency of reduced hydrogen.
[0050] Depending on the hydrocarbon group in the alcohol molecule, the organic alcohol is selected from at least one of fatty alcohols, alicyclic alcohols, and aromatic alcohols; depending on the order of the carbon atom attached to the hydroxyl group, the organic alcohol is selected from primary alcohols or secondary alcohols.
[0051] When the organic alcohol is a primary alcohol, the hydroxyl group in the primary alcohol can be converted into an aldehyde group or a carboxyl group through an electrochemical oxidation reaction.
[0052] When the organic alcohol is a secondary alcohol, the hydroxyl group in the secondary alcohol can be converted into a carbonyl group through an electrochemical oxidation reaction.
[0053] Optionally, the first reaction solvent is selected from at least one of water, methanol, ethanol, acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran, and tert-butanol.
[0054] Considering the hydrogen storage capacity of the hydrogen storage alloy material in the coating, and that excessive hydrogen storage will affect the service life of the hydrogen storage alloy material, the concentration of the organic alcohol in the first reaction substrate is 0.025 mol / L-0.3 mol / L.
[0055] Optionally, the electrolyte is selected from at least one of potassium hydroxide, sodium hydroxide, potassium bicarbonate, potassium carbonate, sodium bicarbonate, and sodium carbonate.
[0056] The anode is selected from a metal electrode, a carbon electrode, a conductive glass electrode, or an electrode supported on an electrochemical catalyst.
[0057] In one embodiment, the current applied to the electrochemical oxidation reaction is 1 mA-500 mA.
[0058] In step S2, after the electrochemical oxidation reaction is completed, the composite cathode storing reduced hydrogen forms a reducing composite cathode, which can self-drive the catalytic hydrogenation reduction reaction without an additional hydrogen source. Washing removes residual reactants adhering to the surface of the reducing composite cathode, preventing the introduction of impurities in subsequent reactions.
[0059] In step S3, the reducing composite cathode, in an organic reaction tank environment containing unsaturated organic matter, uses its own stored reducing hydrogen as a reducing force to catalyze a hydrogenation reduction reaction, causing the unsaturated bonds in the unsaturated organic matter to open and bond with the reducing hydrogen to form hydrogenated organic matter.
[0060] The unsaturated organic compound is selected from at least one of alkyne-based organic compounds, olefin-based organic compounds, and nitro-based organic compounds.
[0061] The second reaction solvent is selected from at least one of water, methanol, ethanol, acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran, and tert-butanol.
[0062] In order to match the reduced hydrogen storage capacity of the reducing composite cathode and achieve efficient catalytic hydrogenation reduction reaction, the concentration of the unsaturated organic compound in the second reaction substrate is 0.02 mol / L-1 mol / L.
[0063] Considering the influence of temperature on the rate of catalytic hydrogenation reduction reaction, the preferred reaction temperature for the catalytic hydrogenation reduction reaction is 20℃-80℃.
[0064] In order to fully release the reducing hydrogen in the reducing composite cathode and ensure the complete reaction of unsaturated organic matter, the reaction time of the catalytic hydrogenation reduction reaction is preferably 4h-20h.
[0065] In step S4, after the reducing composite cathode releases the reduced hydrogen it stores, it is restored to a composite cathode and can be used again in step S1.
[0066] It is evident that steps S1-S4 constitute a closed-loop preparation process, which not only improves the utilization rate of the composite cathode but also significantly enhances the energy utilization efficiency of the electrochemical synthesis reaction system.
[0067] The following specific embodiments will further illustrate the composite cathode and its coupling method for electrochemical oxidation and catalytic hydrogenation reduction reactions.
[0068] Example 1
[0069] The AB5 type mixed rare earth lanthanum-nickel alloy La with a weight ratio of 90:5:5:0.003 was used. 0.8 Ce 0.2 Ni 4.2 Mn 0.6 Al 0.2 A slurry is prepared by mixing carbon black (particle size greater than 100 mesh), PTFE binder, and palladium on carbon catalyst, and coated onto carbon cloth. The mixture is then dried at a constant temperature of 200°C under vacuum for 2 hours to obtain a composite cathode. The La content in the coating of the composite cathode... 0.8 Ce 0.2 Ni 4.2 Mn 0.6 Al 0.2 The lanthanum-nickel alloy loading is 60 mg / cm³. 2 .
[0070] At 20℃, in a 6M potassium hydroxide solution, using nickel foam (effective area 20mm × 20mm) as the anode and a composite cathode of the same effective area, with an Ag / AgCl electrode as the reference electrode, a cyclic activation experiment was conducted at a charge-discharge rate of 0.33C. The cyclic discharge was terminated when the potential of the composite cathode relative to the reference electrode was greater than -0.5V. Figure 2 It can be seen that in a 6M potassium hydroxide solution at 20℃, under the same charging capacity, the discharge capacity of the composite cathode first increases and then remains flat as the number of charge-discharge cycles increases. Furthermore, the composite cathode reaches its maximum discharge capacity of 213mAh / g after the third cycle, indicating that the composite electrode has been fully activated.
[0071] The surface coating contains 240 mg of La 0.8 Ce 0.2 Ni 4.2 Mn 0.6 Al 0.2 A lanthanum-nickel alloy composite cathode (effective area 20mm × 20mm) was placed in an electrolyte containing 0.1 mol / L potassium hydroxide electrolyte, and the anode was nickel foam (effective area 20mm × 20mm). The cathode was operated at 5 mA / cm² at room temperature. 2 An electrochemical oxidation reaction was carried out with an electric current density for 6 hours.
[0072] After the reaction was complete, the composite cathode was removed and simply rinsed in a small amount of aqueous solvent to obtain a reduced composite cathode.
[0073] The reducing composite cathode was transferred to 10 mL of tetrahydrofuran solvent containing 1 mmol of ethyl cinnamate. The reaction flask containing the reducing composite cathode, ethyl cinnamate, and tetrahydrofuran was sealed and placed in a 35°C water bath shaker for 5 h to carry out the catalytic hydrogenation reduction reaction.
[0074] After the reaction was completed, the yield of the hydrogenated product of ethyl cinnamate was tested and found to be 77%.
[0075] Example 2
[0076] The AB5 type mixed rare earth lanthanum-nickel alloy La with a weight ratio of 90:5:5:0.003 was used. 0.7 Ce 0.3 Ni 3.9 Mn 0.4 Al 0.3 Co 0.4 A slurry is prepared by mixing carbon black (particle size greater than 100 mesh), PTFE binder, and palladium on carbon catalyst, and coated onto carbon cloth. The mixture is then dried at a constant temperature of 200°C under vacuum for 2 hours to obtain a composite cathode. The La content in the coating of the composite cathode... 0.7 Ce 0.3 Ni 3.9 Mn 0.4 Al 0.3 Co 0.4 The lanthanum-nickel alloy loading is 60 mg / cm³. 2 .
[0077] At a temperature of 20℃, in a 6M potassium hydroxide solution, using nickel foam (effective area 20mm×20mm) as the anode, a composite cathode with the same effective area, and an Ag / AgCl electrode as the reference electrode, a cyclic activation experiment was conducted at a charge-discharge rate of 0.33C. The cyclic discharge was terminated when the potential of the composite cathode relative to the reference electrode was greater than -0.5V.
[0078] The surface coating contains 240 mg of La 0.7 Ce 0.3 Ni 3.9 Mn 0.4 Al 0.3 Co 0.4 A lanthanum-nickel alloy composite cathode (effective area 20mm × 20mm) was placed in an electrolyte containing 0.1 mol / L potassium hydroxide electrolyte, and the anode was nickel foam (effective area 20mm × 20mm). The cathode was operated at 5 mA / cm² at room temperature. 2 An electrochemical oxidation reaction was carried out with an electric current density for 6 hours.
[0079] After the reaction was complete, the composite cathode was removed and simply rinsed in a small amount of aqueous solvent to obtain a reduced composite cathode.
[0080] The reducing composite cathode was transferred to 10 mL of tetrahydrofuran solvent containing 1 mmol of ethyl cinnamate. The reaction flask containing the reducing composite cathode, ethyl cinnamate, and tetrahydrofuran was sealed and placed in a 35°C water bath shaker for 5 hours to carry out the catalytic hydrogenation reduction reaction.
[0081] After the reaction was completed, the yield of the hydrogenated product of ethyl cinnamate was tested and found to be 74%.
[0082] Example 3
[0083] The AB5 type mixed rare earth lanthanum-nickel alloy La with a weight ratio of 90:5:5:0.003 was used. 0.8 Ce 0.2 Ni 3.7 Mn 0.4 Al 0.2 Co 0.7 A slurry is prepared by mixing carbon black (particle size greater than 100 mesh), PTFE binder, and palladium on carbon catalyst, and coated onto carbon cloth. The mixture is then dried at a constant temperature of 200°C under vacuum for 2 hours to obtain a composite cathode. The La content in the coating of the composite cathode... 0.8 Ce 0.2 Ni 3.7 Mn 0.4 Al 0.2 Co 0.7 The lanthanum-nickel alloy loading is 60 mg / cm³. 2 .
[0084] At a temperature of 20℃, in a 6M potassium hydroxide solution, using nickel foam (effective area 20mm×20mm) as the anode, a composite cathode with the same effective area, and an Ag / AgCl electrode as the reference electrode, a cyclic activation experiment was conducted at a charge-discharge rate of 0.33C. The cyclic discharge was terminated when the potential of the composite cathode relative to the reference electrode was greater than -0.5V.
[0085] The surface coating contains 240 mg of La 0.8 Ce 0.2 Ni 3.7 Mn 0.4 Al 0.2 Co 0.7 A lanthanum-nickel alloy composite cathode (effective area 20mm × 20mm) was placed in an electrolyte containing 0.1 mol / L potassium hydroxide electrolyte, and the anode was nickel foam (effective area 20mm × 20mm). The cathode was operated at 5 mA / cm² at room temperature. 2 An electrochemical oxidation reaction was carried out with an electric current density for 6 hours.
[0086] After the reaction was complete, the composite cathode was removed and simply rinsed in a small amount of aqueous solvent to obtain a reduced composite cathode.
[0087] The reducing composite cathode was transferred to 10 mL of tetrahydrofuran solvent containing 1 mmol of ethyl cinnamate. The reaction flask containing the reducing composite cathode, ethyl cinnamate, and tetrahydrofuran was sealed and placed in a 35°C water bath shaker for 5 hours to carry out the catalytic hydrogenation reduction reaction.
[0088] After the reaction was completed, the yield of the hydrogenated product of ethyl cinnamate was tested to be 53%.
[0089] Example 4
[0090] The AB5 type mixed rare earth lanthanum-nickel alloy La with a weight ratio of 90:5:5:0.003 was used. 0.8 Ce 0.2 Ni 4.2 Mn 0.6 Al 0.2 A slurry is prepared by mixing carbon black (particle size greater than 100 mesh), PTFE binder, and palladium-on-carbon catalyst, and coated onto carbon cloth. The mixture is then dried at a constant temperature of 150°C under vacuum for 2 hours to obtain a composite cathode. The La content in the coating of the composite cathode... 0.8 Ce 0.2 Ni 4.2 Mn 0.6 Al 0.2 The lanthanum-nickel alloy loading is 50 mg / cm³. 2 .
[0091] At a temperature of 20℃, in a 6M potassium hydroxide solution, using nickel foam (effective area 20mm×20mm) as the anode, a composite cathode with the same effective area, and an Ag / AgCl electrode as the reference electrode, a cyclic activation experiment was conducted at a charge-discharge rate of 0.33C. The cyclic discharge was terminated when the potential of the composite cathode relative to the reference electrode was greater than -0.5V.
[0092] The surface coating contains 200mg of La0.7 Ce 0.3 Ni 3.9 Mn 0.4 Al 0.3 Co 0.4 A lanthanum-nickel alloy composite cathode (effective area 20mm × 20mm) was placed in an electrolyte containing 0.1 mol / L potassium hydroxide electrolyte, and the anode was nickel foam (effective area 20mm × 20mm). The cathode was operated at 5 mA / cm² at room temperature. 2 An electrochemical oxidation reaction was carried out with an electric current density for 6 hours.
[0093] After the reaction was complete, the composite cathode was removed and simply rinsed in a small amount of aqueous solvent to obtain a reduced composite cathode.
[0094] The reducing composite cathode was transferred to 10 mL of tetrahydrofuran solvent containing 1 mmol of ethyl cinnamate. The reaction flask containing the reducing composite cathode, ethyl cinnamate, and tetrahydrofuran was sealed and placed in a 35°C water bath shaker for 5 hours to carry out the catalytic hydrogenation reduction reaction.
[0095] After the reaction was completed, the yield of the hydrogenated product of ethyl cinnamate was tested and found to be 60%.
[0096] Example 5
[0097] The AB5 type mixed rare earth lanthanum-nickel alloy La with a weight ratio of 90:5:5:0.003 was used. 0.8 Ce 0.2 Ni 4.2 Mn 0.6 Al 0.2 A slurry is prepared by mixing carbon black (particle size greater than 100 mesh), PTFE binder, and palladium-on-carbon catalyst, and coated onto carbon cloth. The mixture is then dried at a constant temperature of 150°C under vacuum for 2 hours to obtain a composite cathode. The La content in the coating of the composite cathode... 0.8 Ce 0.2 Ni 4.2 Mn 0.6 Al 0.2 The lanthanum-nickel alloy loading is 80 mg / cm³. 2 .
[0098] At a temperature of 20℃, in a 6M potassium hydroxide solution, using nickel foam (effective area 20mm×20mm) as the anode, a composite cathode with the same effective area, and an Ag / AgCl electrode as the reference electrode, a cyclic activation experiment was conducted at a charge-discharge rate of 0.33C. The cyclic discharge was terminated when the potential of the composite cathode relative to the reference electrode was greater than -0.5V.
[0099] The surface coating contains 240 mg of La 0.8 Ce 0.2 Ni3.7 Mn 0.4 Al 0.2 Co 0.7 A lanthanum-nickel alloy composite cathode (effective area 20mm × 20mm) was placed in an electrolyte containing 0.1 mol / L potassium hydroxide electrolyte, and the anode was nickel foam (effective area 20mm × 20mm). The cathode was operated at 5 mA / cm² at room temperature. 2 An electrochemical oxidation reaction was carried out with an electric current density for 6 hours.
[0100] After the reaction was complete, the composite cathode was removed and simply rinsed in a small amount of aqueous solvent to obtain a reduced composite cathode.
[0101] The reducing composite cathode was transferred to 10 mL of tetrahydrofuran solvent containing 1 mmol of ethyl cinnamate. The reaction flask containing the reducing composite cathode, ethyl cinnamate, and tetrahydrofuran was sealed and placed in a 35°C water bath shaker for 5 hours to carry out the catalytic hydrogenation reduction reaction.
[0102] After the reaction was completed, the yield of the hydrogenated product of ethyl cinnamate was tested and found to be 69%.
[0103] Example 6
[0104] The composite cathode was prepared according to Example 1.
[0105] At a temperature of 20℃, in a 6M potassium hydroxide solution, using nickel foam (effective area 20mm×20mm) as the anode, a composite cathode with the same effective area, and an Ag / AgCl electrode as the reference electrode, a cyclic activation experiment was conducted at a charge-discharge rate of 0.33C. The cyclic discharge was terminated when the potential of the composite cathode relative to the reference electrode was greater than -0.5V.
[0106] Using nickel hydroxide / nickel foam (effective area 20mm×20mm) as the anode, and loaded with 240mg La 0.8 Ce 0.2 Ni 4.2 Mn 0.6 Al 0.2 A lanthanum-nickel alloy composite cathode (effective area 20mm × 20mm) was used as the cathode. 0.75 mmol of benzyl alcohol, 0.1 mol / L potassium hydroxide electrolyte, and 30 mL of a tert-butanol / water mixed reaction solvent (1:1) were added to a diaphragm-free electrolytic cell. The reaction was carried out at 5 mA / cm² at room temperature. 2 The alcohol electrochemical oxidation reaction was carried out with an electric current density for 6 hours.
[0107] After the reaction was completed, the composite cathode was removed and rinsed in a small amount of tert-butanol / water mixed solvent to obtain a reduced composite cathode.
[0108] The reducing composite cathode was transferred to 10 mL of tetrahydrofuran solvent containing 0.5 mmol of ethyl cinnamate. The reaction flask containing the reducing composite cathode, ethyl cinnamate, and tetrahydrofuran was sealed and placed in a 35°C water bath shaker for 5 hours to carry out the catalytic hydrogenation reduction reaction.
[0109] The washing solution was mixed with the reaction solution for the electrochemical oxidation of alcohol, and the electrolytic cell and anode were cleaned with a small amount of solvent. The washing solution and reaction solution were then combined. 0.0145 g of internal standard tricresylbenzene was added, and an appropriate amount of 1 mol / L hydrochloric acid solution was added dropwise to adjust the pH of the reaction solution to slightly acidic. 1 mL of the liquid was analyzed by liquid chromatography, revealing a 100% conversion rate for benzyl alcohol oxidation, a 1% yield of benzaldehyde, and a 97% yield of benzoic acid.
[0110] After the catalytic hydrogenation reduction reaction was completed, the composite cathode was removed from the hydrogenation reaction solution and cleaned with a small amount of tetrahydrofuran solvent. The cleaning solution and the reaction solution were combined, and 0.0157 g of internal standard methyltrimethylbenzene was added. 1 mL of the liquid was taken for gas chromatography analysis, and the reaction conversion rate of ethyl cinnamate was 100%, while the yield of the hydrogenation product of ethyl cinnamate was 94%. The mismatch between the conversion rate and the yield was due to the presence of a small amount of hydrolyzed ethyl cinnamate.
[0111] The composite cathode, after the catalytic hydrogenation reduction reaction, was reactivated and used in a coupled experiment of alcohol electrochemical oxidation and catalytic hydrogenation reduction. One activation and the coupled experiment of alcohol electrochemical oxidation and catalytic hydrogenation reduction were considered one coupled experimental cycle. After 10 coupled experimental cycles, there were no significant changes in the yield of alcohol oxidation and the hydrogenation yield of ethyl cinnamate. Furthermore, according to... Figure 3 and Figure 4 Comparing the scanning electron microscope images of the composite cathode coating before the reaction and after 5 coupling experimental cycles, it can be seen that the morphology of the composite cathode coating did not change significantly after 5 coupling experimental cycles, proving that the composite cathode coating has good chemical stability.
[0112] Example 7
[0113] The composite cathode was prepared according to Example 1.
[0114] At a temperature of 20℃, in a 6M potassium hydroxide solution, using nickel foam (effective area 20mm×20mm) as the anode, a composite cathode with the same effective area, and an Ag / AgCl electrode as the reference electrode, a cyclic activation experiment was conducted at a charge-discharge rate of 0.33C. The cyclic discharge was terminated when the potential of the composite cathode relative to the reference electrode was greater than -0.5V.
[0115] Using nickel hydroxide / nickel foam (effective area 20mm×20mm) as the anode, and loaded with 240mg La0.8 Ce 0.2 Ni 4.2 Mn 0.6 Al 0.2 A lanthanum-nickel alloy composite cathode (effective area 20mm × 20mm) was used as the cathode. 0.75 mmol of benzyl alcohol, 0.1 mol / L potassium hydroxide electrolyte, and 30 mL of a tert-butanol / water mixed reaction solvent (1:1) were added to a diaphragm-free electrolytic cell. The reaction was carried out at 5 mA / cm² at room temperature. 2 The alcohol electrochemical oxidation reaction was carried out with an electric current density for 6 hours.
[0116] After the reaction was completed, the composite cathode was removed and rinsed in a small amount of tert-butanol / water mixed solvent to obtain a reduced composite cathode.
[0117] The reducing composite cathode was transferred to 10 mL of methanol containing 0.7 mmol of cinnamamide. The reaction flask containing the reducing composite cathode, cinnamamide, and methanol was sealed and placed in a 35°C water bath shaker for 7 h to carry out the catalytic hydrogenation reduction reaction.
[0118] The washing solution was mixed with the reaction solution for the electrochemical oxidation of alcohol, and the electrolytic cell and anode were cleaned with a small amount of solvent. The washing solution and reaction solution were then combined. 0.0167 g of internal standard tricresylbenzene was added, and an appropriate amount of 1 mol / L hydrochloric acid solution was added dropwise to adjust the pH of the reaction solution to slightly acidic. 1 mL of the liquid was analyzed by liquid chromatography, revealing a 100% conversion rate for benzyl alcohol oxidation, a 2% yield of benzaldehyde, and a 96% yield of benzoic acid.
[0119] After the catalytic hydrogenation reduction reaction was completed, the composite cathode was removed from the hydrogenation reaction solution and cleaned with a small amount of methanol solvent. The cleaning solution and the reaction solution were combined, and 0.0168 g of internal standard methyltrimethylbenzene was added. 1 mL of the liquid was taken for gas chromatography analysis, and the reaction conversion rate of cinnamamide was 100%, and the yield of cinnamamide hydrogenation product was 98%.
[0120] Comparative Example 1
[0121] The difference between Comparative Example 1 and Example 1 is that the La in the composite cathode surface coating... 0.8 Ce 0.2 Ni 4.2 Mn 0.6 Al 0.2 The lanthanum-nickel alloy loading is 20 mg / cm³. 2 .
[0122] The yield of the hydrogenated product of ethyl cinnamate was 10% according to the test.
[0123] Comparative Example 2
[0124] The difference between Comparative Example 2 and Example 1 is that the La in the composite cathode surface coating... 0.8 Ce 0.2 Ni 4.2 Mn 0.6 Al 0.2 The lanthanum-nickel alloy loading is 100 mg / cm³. 2 .
[0125] Tests showed that the yield of hydrogenated products of ethyl cinnamate was 50%. This is because, with the weight ratio remaining constant, the increase in alloy loading led to a corresponding increase in the content of other additives, resulting in an excessively thick coating and a weakened ability to chemically adsorb hydrogen.
[0126] Comparative Example 3
[0127] The difference between Comparative Example 3 and Example 1 is that LaNi5 alloy material was used.
[0128] The yield of hydrogenation products of ethyl cinnamate was 2% according to the test. This is because the LaNi5 alloy has difficulty in stably storing hydrogen under normal pressure, resulting in poor hydrogenation catalytic performance.
[0129] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0130] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A method for coupling electrochemical oxidation reactions with catalytic hydrogenation reduction reactions, the method comprising: providing a substrate comprising a metal oxide; providing a catalyst comprising a metal; and exposing the substrate to the catalyst under conditions effective to produce a metal oxide and a metal hydride. The coupling method includes the following steps: Organic alcohol, electrolyte and first reaction solvent are mixed to form the first reaction substrate, which is added to the electrolytic cell. After the composite cathode is activated, it is placed in the electrolytic cell together with the anode. Electrochemical oxidation reaction is carried out by passing electricity to obtain aldehyde, ketone or acid. After the electrochemical oxidation reaction is completed, the composite cathode is removed from the electrolytic cell and rinsed to obtain a reducing composite cathode; Unsaturated organic compounds are mixed with a second reaction solvent to form a second reaction substrate, which is then added to an organic reaction tank and placed in the reducing composite cathode for catalytic hydrogenation reduction to obtain hydrogenated organic compounds. After the catalytic hydrogenation reduction reaction is completed, a composite cathode is obtained, and the composite cathode after the catalytic hydrogenation reduction reaction can be reactivated. The composite cathode includes a current collector and a coating disposed on the current collector. The coating material includes a hydrogen storage alloy material, a conductive agent, and a binder. The hydrogen storage alloy material has a loading of 40 mg / cm² on the current collector. 2 -80mg / cm 2 .
2. The method of coupling electrochemical oxidation reactions with catalytic hydrogenation reductions of claim 1, wherein, The hydrogen storage alloy material is selected from AB5 type hydrogen storage alloy material, AB2 type hydrogen storage alloy material, AB type hydrogen storage alloy material or A2B type hydrogen storage alloy material.
3. The method of coupling electrochemical oxidation reactions with catalytic hydrogenation reductions of claim 1, wherein, The conductive agent is selected from at least one of carbon black, copper powder, and nickel powder, and the mass ratio of the conductive agent to the hydrogen storage alloy material is 1:10-1:
100. And / or, the binder is selected from at least one of polytetrafluoroethylene, water-soluble rubber, and cellulose, and the mass ratio of the binder to the hydrogen storage alloy material is 1:10 to 1:
100.
4. The method of coupling electrochemical oxidation reactions with catalytic hydrogenation reductions according to any one of claims 1 to 3, characterized in that, The coating material also includes a catalyst, which is selected from at least one of noble metals, metal oxides, and metal sulfides, and the mass ratio of the catalyst to the hydrogen storage alloy material is less than or equal to 1:
100.
5. The method of coupling electrochemical oxidation reactions with catalytic hydrogenative reductions of claim 1, wherein, The activation method of the composite cathode includes: performing a constant current charge-discharge cycle experiment on the composite cathode in a potassium hydroxide solution.
6. The method of coupling electrochemical oxidation reactions with catalytic hydrogenative reductions of claim 1, wherein, The organic alcohol is selected from at least one of fatty alcohols, alicyclic alcohols, and aromatic alcohols; And / or, the first reaction solvent is selected from at least one of water, methanol, ethanol, acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran, and tert-butanol.
7. The method of coupling electrochemical oxidation reactions with catalytic hydrogenative reductions of claim 1, wherein, The concentration of the organic alcohol in the first reaction substrate is 0.025 mol / L to 0.3 mol / L.
8. The method of coupling electrochemical oxidation reactions with catalytic hydrogenative reductions of claim 1, wherein, The unsaturated organic compound is selected from at least one of alkyne-based organic compounds, olefin-based organic compounds, and nitro-based organic compounds; And / or, the second reaction solvent is selected from at least one of water, methanol, ethanol, acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran, and tert-butanol.
9. The coupling method of electrochemical oxidation reaction and catalytic hydrogenation reduction reaction according to claim 1, characterized in that, The concentration of the unsaturated organic compound in the second reaction substrate is 0.02 mol / L to 1 mol / L.
Citation Information
Patent Citations
Hydrogen storage alloy electrode and manufacture thereof
JP1992104462A
Method for hydrogenating and reducing cyclic organic compound
JP1994056702A