A semiconductor thin film forming method, semiconductor structure and memory

By adsorbing precursors on the sidewalls of DRAM bit lines and using plasma to deposit oxynitride intermediate phases, the problem of large dielectric constants and stress of Si3N4 and SiO2 is solved, parasitic capacitance is reduced, and DRAM performance is improved.

CN116133367BActive Publication Date: 2024-10-22CHANGXIN MEMORY TECH INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202110925579.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-12
Publication Date
2024-10-22
Estimated Expiration
2041-08-12

AI Technical Summary

Technical Problem

The dielectric constants of Si3N4 and SiO2 in the existing DRAM bit line sidewall structure are large, resulting in large parasitic capacitance, which affects DRAM performance. At the same time, Si3N4 has large stress and poor contact with SiO2, which affects memory performance.

Method used

By adsorbing the precursor on the semiconductor substrate and depositing the first film and the second film using a plasma reaction containing oxygen ions and nitrogen ions, a nitride oxide intermediate phase is formed to reduce the parasitic capacitance at the interface between the nitride and the oxide, and The first film and the second film are alternately deposited in the same process to reduce parasitic capacitance.

Benefits of technology

It effectively reduces the parasitic capacitance at the interface between nitride and oxide, alleviates the problem of poor contact between Si3N4 and SiO2, and improves memory performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116133367B_ABST
    Figure CN116133367B_ABST
Patent Text Reader

Abstract

The embodiments of the present application disclose a method for forming a semiconductor thin film, a semiconductor structure and a memory. The method includes: introducing a precursor into a chamber, the precursor is adsorbed on a semiconductor substrate; purging the chamber to remove the unadsorbed precursor; introducing a plasma containing oxygen ions and nitrogen ions into the chamber, and reacting with the precursor to deposit a first thin film; purging the chamber to remove the unreacted plasma; introducing a plasma containing oxygen ions into the chamber, and reacting with the precursor adsorbed on the semiconductor substrate to deposit a second thin film; cyclically performing the above steps until the total thickness of the first film and the second film reaches a predetermined value. The present application effectively reduces the parasitic capacitance of the nitride and oxide interface by forming the first film and the second film on the semiconductor substrate, thereby alleviating the technical problem of poor contact.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor process technology, and more specifically, to a semiconductor thin film forming method, a semiconductor structure and a memory. Background Art

[0002] In the field of semiconductor production, during the interconnection manufacturing process of deep trench DRAM (Dynamic Random Access Memory), the bit line sidewall formation process is as follows: Figure 1(A) to Figure 1(E) First, Si is deposited on the bit line. 3 N 4 As a barrier layer and a stop layer for chemical mechanical polishing. Secondly, a layer of SiO with a thickness of less than 5nm is deposited by ALD (Atomic Layer Deposition) technology. 2 As a connection layer, it can make dense contact with the DHPS (polyhydrogenated polysilane) filled in later. Finally, a complete bit line sidewall is formed by chemical mechanical polishing and etching.

[0003] In the existing DRAM bit line sidewall structure, the Si 3 N 4 and SiO 2 Two layers. Among them, Si 3 N 4 The structure is compact and the anti-diffusion ability is strong, so it can be used as an excellent barrier layer, but Si 3 N 4 The dielectric constant of Si is large, and the parasitic capacitance generated is large, which affects the performance of DRAM. 3 N 4 The stress is large and there is 2 Poor contact situation. Summary of the invention

[0004] In view of this, the purpose of the embodiments of the present application is to provide a semiconductor thin film forming method, a semiconductor structure and a memory to alleviate the existing technical problems.

[0005] According to some embodiments, the first aspect of the present application provides a method for forming a semiconductor thin film, which includes: introducing a precursor into a chamber, the precursor being adsorbed on a semiconductor substrate; purging the chamber to remove unadsorbed precursor; introducing a plasma containing oxygen ions and nitrogen ions into the chamber, and reacting with the precursor to deposit a first thin film; purging the chamber to remove unreacted plasma; introducing a plasma containing oxygen ions into the chamber, and reacting with the precursor adsorbed on the semiconductor substrate to deposit a second thin film; and cyclically performing the above steps until the total thickness of the first thin film and the second thin film reaches a predetermined value.

[0006] According to some embodiments, the second aspect of the present application provides a semiconductor structure, comprising a first thin film and a second thin film formed by the semiconductor thin film formation method of the first aspect of the present application, including: a first deposition layer and a second deposition layer formed on a semiconductor substrate, the first deposition layer being a stop layer for chemical mechanical polishing, and the second deposition layer being formed by alternating the first film and the second film.

[0007] According to some embodiments, the third aspect of the present application provides a memory, comprising a first thin film and a second thin film formed by the semiconductor thin film forming method of the first aspect of the present application, including: a first deposition layer and a second deposition layer formed on the side wall of the memory bit line, the first deposition layer is a stop layer for chemical mechanical polishing, and the second deposition layer is formed by alternating the first film and the second film

[0008] The embodiments of the present disclosure can / at least have the following advantages: a first thin film is deposited by reacting a plasma containing oxygen ions and nitrogen ions with a precursor adsorbed on a semiconductor substrate, wherein the first thin film is a nitride oxide containing nitrogen and oxygen elements. The first thin film is an intermediate phase between nitride and oxide, and can effectively reduce the parasitic capacitance at the interface between nitride and oxide, thereby alleviating the technical problem of poor contact; thereafter, a second thin film is deposited by reacting a plasma containing oxygen ions with a precursor adsorbed on a semiconductor substrate, thereby achieving the deposition of the first thin film and the second thin film in the same process. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] 1(A) to 1(E) are schematic diagrams of a process for forming a side wall of a memory bit line in the prior art;

[0010] FIG. 1(A) is a schematic diagram of a memory bit line without forming a sidewall, and FIG. 1(B) is a schematic diagram of FIG. 1(A) after Si is deposited by ALD. 3 N 4 1(C) is a schematic diagram of a memory bit line of FIG. 1(B) after ALD deposition of SiO 2 FIG1(D) is a schematic diagram of the memory bit line of FIG1(C) after SOD (Spin-on Dielectrics), and FIG1(E) is a schematic diagram of the memory bit line of FIG1(D) after chemical mechanical polishing and etching.

[0011] Figure 2 This is a schematic flow chart of a semiconductor thin film forming method according to an embodiment of the present application;

[0012] Figure 3 This is a timing diagram of a thin film forming process of a semiconductor thin film forming method according to an embodiment of the present application;

[0013] 4(A) to 4(E) are schematic diagrams of a thin film forming process of a semiconductor thin film forming method according to an embodiment of the present application;

[0014] Among them, Figure 4(A) is a schematic diagram of a semiconductor structure memory bit line without forming a sidewall film, Figure 4(B) is a schematic diagram of a semiconductor structure memory bit line after the first deposition layer is formed in Figure 4(A), Figure 4 (C) is a schematic diagram of a semiconductor structure memory bit line after the second deposition layer is formed in Figure 4(B), Figure 4 (D) is a schematic diagram of a semiconductor structure memory bit line after chemical mechanical grinding and etching in Figure 4(C), and Figure 4(E) is a partial enlarged view of Figure 4(D).

[0015] Figure 5 This is a semiconductor thin film forming method according to an embodiment of the present application. 2 With N 2 Schematic diagram of the effect of gas flow ratio on parasitic capacitance of semiconductor devices;

[0016] Figure 6 It is a schematic diagram of the effect of the thickness ratio of the first deposition layer and the second deposition layer on the parasitic capacitance of a semiconductor device in a semiconductor thin film forming method according to an embodiment of the present application;

[0017] Figure 7 This is a schematic diagram of a semiconductor structure according to an embodiment of the present application;

[0018] Figure 8 It is a schematic diagram of a memory structure of an embodiment of the present application.

[0019] Reference numerals:

[0020] 11: bit line insulation layer; 21: bit line middle layer; 31: bit line conductive layer; 41: Si 3 N 4 Layer; 1: bit line insulation layer; 2: bit line intermediate layer; 3: bit line conductive layer; 4: Si 3 N 4 Layer; 5: SiO 2 Layer; 6: SOD schematic; 7: second deposition layer; 71: first film; 72: second film; 10: precursor introduction; 20: chamber purge; 30: plasma containing nitrogen ions and oxygen ions introduction; 40: radio frequency signal; 50: plasma containing oxygen ions introduction; 100: semiconductor substrate. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is further described in detail below in conjunction with specific implementations and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present application. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concepts of the present application.

[0022] The schematic diagram of the layer structure according to the embodiment of the present application is shown in the accompanying drawings. These figures are not necessarily drawn to scale, and some details are magnified and some details may be omitted for the purpose of clarity. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships therebetween are only exemplary, and may deviate in practice due to manufacturing tolerances or technical limitations, and those skilled in the art may further design regions / layers with different shapes, sizes, and relative positions according to actual needs.

[0023] Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application. The present application will be described in more detail below with reference to the accompanying drawings. In each of the drawings, the same elements are represented by similar reference numerals. For clarity, the various parts in the drawings are not drawn to scale.

[0024] 1(A) to 1(E) are schematic diagrams of a process for forming a side wall of a memory bit line in the prior art.

[0025] FIG. 1(A) is a schematic diagram of a memory bit line without forming a sidewall, and FIG. 1(B) is a schematic diagram of FIG. 1(A) after Si is deposited by ALD. 3 N 4 1(C) is a schematic diagram of a memory bit line of FIG. 1(B) after ALD deposition of SiO 2 FIG1(D) is a schematic diagram of the memory bit line of FIG1(C) after SOD (Spin-On Dielectrics), and FIG1(E) is a schematic diagram of the memory bit line of FIG1(D) after chemical mechanical polishing and etching.

[0026] Referring to FIG. 1(A), the memory bit line is composed of a bit line insulating layer 10, a bit line intermediate layer 20 and a bit line conductive layer 30. In FIG. 1(B), the memory bit line is deposited by the ALD process to form a Si 3 N 4 In FIG1(C), the memory bit line is deposited by the ALD process to form SiO 2 Layer 5. After gap filling 6 through SOD in FIG1 (D), the complete memory bit line sidewall in FIG1 (E) is formed by chemical mechanical polishing and etching. Referring to FIG1 (E), the complete memory bit line sidewall includes Si 3 N 4 Layer 41 and SiO 2 Layer 5.

[0027] It should be noted that chemical mechanical polishing (CMP) is also called chemical mechanical polishing. Its principle is a processing technology that combines chemical corrosion and mechanical removal. It is a technology that can achieve global surface flattening in mechanical processing. Etching is a technology that removes materials by chemical reaction or physical impact.

[0028] Si 3 N 4 The structure is compact and the anti-diffusion ability is strong, so it can be used as an excellent barrier layer. However, Si 3 N 4 The dielectric constant of Si is large, and the parasitic capacitance generated is large, which affects the performance of the memory. 3 N 4 The stress is greater than that of SiO 2 There is a poor contact surface. Parasitic capacitance generally refers to the capacitance characteristics of non-capacitive devices under high frequency conditions. DRAM relies on the charging and discharging of internal parasitic capacitance to memorize information. A charged capacitor is a logic 1, and an uncharged capacitor is a logic 0. However, on the other hand, as the frequency of DRAM continues to increase, the influence of lead parasitic inductance and parasitic capacitance becomes more serious, causing greater electrical stress on the device, which is specifically manifested as overvoltage and overcurrent glitches. For DRAM, large parasitic capacitance will affect DRAM performance. Therefore, Si in Figure 1 (E) 3 N 4 Layer 41 and SiO 2 Layer 5 makes the memory bit line parasitic capacitance large, and Si 3 N 4 Layer 41 and SiO 2 Layer 5 has a poor contact surface.

[0029] Figure 2 It is a schematic flow chart of a semiconductor thin film forming method according to an embodiment of the present application.

[0030] like Figure 2 As shown, the semiconductor thin film forming method provided in the embodiment of the present application mainly includes 7 steps, and the 7 steps are described in detail below.

[0031] Step S1, adsorbing a precursor onto a semiconductor substrate.

[0032] Specifically, a precursor is introduced into the chamber, and the precursor is adsorbed on the semiconductor substrate. It should be noted that in the field of semiconductor preparation technology, a precursor is a precursor product that can achieve a target product after certain steps, and the precursor is the basis of the ALD deposition process. The first step of both ALD and PEALD (Plasma Enhanced Atomic Layer Deposition) is to adsorb or saturate the reaction precursor on the semiconductor substrate.

[0033] In some embodiments, the precursor is a compound or mixture of silicon and hydrogen. For example, it can be silane (SiH 4 , silicon tetrahydride), silane is a colorless gas that can be adsorbed on semiconductor substrates.

[0034] In some embodiments, the compound of silicon and hydrogen is selected from any one of tetrakis(dimethylamino)silane (TDMAS), isopropylaminosilane (DIPAS), bis(diethylamide)silane (BDEAS), bis(tert-butylamino)silane (BTBAS), or any combination thereof. In some embodiments, the compound of silicon and hydrogen is selected from bis(diethylamide)silane (BDEAS).

[0035] In step S1 of some embodiments, the adsorption time of the precursor and the semiconductor substrate is set to 2-10 seconds. Setting the length of the adsorption time can ensure the adsorption degree of the precursor in the substrate. For example, when the adsorption time is greater than a certain value, the precursor is saturatedly adsorbed.

[0036] Step S2, purging the chamber to remove the unadsorbed precursor.

[0037] In the ALD or PEALD thin film deposition process, if the unadsorbed precursor is not purged out of the chamber, the unadsorbed precursor will react with the subsequently introduced reactants, thereby affecting the reaction of the adsorbed precursor and affecting the thin film deposition process of the adsorbed precursor.

[0038] In an optional embodiment, an inert gas is used to purge the chamber. Optionally, an inert gas argon (Ar) is introduced to purge and remove excess precursor. It should be noted that the gas used to purge and remove excess precursor cannot react with the precursor, so an inert gas is selected. In addition, any gas that does not react with the precursor can be used to purge excess precursor.

[0039] Step S3, reacting to form a first thin film.

[0040] Specifically, plasma containing oxygen ions and nitrogen ions is introduced into the chamber and reacts with the precursor adsorbed on the semiconductor substrate to deposit the first film.

[0041] It should be noted that the reaction of ALD or PEALD is self-limiting, that is, the precursor is input into the semiconductor substrate and is retained on the surface by adsorption or saturated adsorption; when the subsequent reactants are introduced into the reaction chamber, they will react with the precursor adsorbed on the surface of the semiconductor substrate. A replacement reaction will occur between the precursor and the reactants and corresponding by-products will be produced until the precursor on the surface of the semiconductor substrate is completely consumed, the reaction will automatically stop and the required atomic layer film will be deposited on the surface of the semiconductor substrate.

[0042] In some embodiments, the precursor is a compound of silicon and hydrogen, and a plasma containing oxygen ions and nitrogen ions is introduced into the chamber. The plasma containing oxygen ions and nitrogen ions reacts with the compound of silicon and hydrogen to generate silicon oxynitride SiON.

[0043] In some embodiments, the plasma containing oxygen ions and nitrogen ions is formed by a gas flow ratio of 1:1 to 1:20 of O 2 With N 2 or NH 3 Optionally, the plasma is generated by O 2 With N 2 or NH 3 Reactive gases such as , are generated in the plasma reaction chamber and then introduced into the chamber to react with the precursor. For example, the plasma is excited by a radio frequency generator. 2 With N 2 or NH 3 In one embodiment, O 2 With N 2 The gas flow ratio is 1:9. By controlling the O 2 With N 2 or NH 3 The ratio of nitrogen to oxygen elements in the first film is precisely controlled by adjusting the plasma source flow ratio to control the magnitude of the generated parasitic capacitance.

[0044] In some embodiments, the plasma is set to be passed for 1-10 seconds. 2 When the plasma is generated, the plasma introduction time is set to 5 seconds. It should be noted that the plasma content in the chamber is different when the plasma introduction time is different.

[0045] In step S4, the chamber is purged to remove unreacted plasma.

[0046] Likewise, in order to prevent the unreacted plasma from reacting with the reactive substances introduced in the subsequent process, the unreacted plasma needs to be purged out of the chamber.

[0047] In an optional embodiment, an inert gas is used to purge the chamber. Optionally, an inert gas argon (Ar) is introduced to purge and remove unreacted plasma. It should be noted that the gas used to purge and remove unreacted plasma cannot react with the plasma, so an inert gas is selected. In addition, any gas that does not react with the plasma and the first film can be used to purge the unreacted plasma.

[0048] Step S5, reacting to form a second thin film.

[0049] Specifically, steps S1 and S2 are performed to introduce plasma containing oxygen ions into the chamber to react with the precursor adsorbed on the semiconductor substrate to deposit the second film.

[0050] In some embodiments, the precursor is a compound of silicon and hydrogen, and a plasma containing oxygen ions is introduced into the chamber, and the plasma containing oxygen ions reacts with the compound of silicon and hydrogen to generate silicon dioxide SiO 2 .

[0051] Optionally, in step S5, the precursor adsorption time is set to 3 seconds.

[0052] In some embodiments, in steps S3 and S5, during the deposition phases of the first thin film and the second thin film, the temperature of the chamber is set to 40° C. to 110° C.

[0053] Step S6, executing step S4. After the second film deposition is completed, executing step S4, blowing unreacted plasma out of the chamber.

[0054] Step S7, returning to step S1, and cyclically executing the above steps until the total thickness of the first film and the second film reaches a predetermined value.

[0055] Figure 3 It is a timing diagram of a thin film forming process of a semiconductor thin film forming method according to an embodiment of the present application.

[0056] like Figure 3 As shown, one process cycle includes two stages: first thin film deposition and second thin film deposition. In the first thin film deposition stage, there are four stages: precursor introduction 10, chamber purge 20, plasma introduction 30 containing nitrogen ions and oxygen ions, and chamber purge 20, and each stage is performed in chronological order.

[0057] In the second film deposition stage, there are four stages, namely, the introduction of precursor 10, chamber purging 20, the introduction of plasma containing oxygen ions 50, and chamber purging 20. Each stage is performed in chronological order. Optionally, the plasma is excited by a radio frequency signal, so in the gas O 2 With N 2 or NH 3During the passage, the RF signal 40 excites O 2 With N 2 or NH 3 A plasma containing ions and oxygen ions, or a plasma containing oxygen ions, is generated.

[0058] refer to Figure 3 In some embodiments, steps S1 to S7 are repeated until the total thickness of the first film and the second film reaches a predetermined value, that is, multiple process cycles are repeated to deposit the first film and the second film of the expected thickness. It should be noted that ALD or PEALD has higher control accuracy than conventional deposition processes such as metal organic chemical vapor deposition, molecular beam epitaxy and physical vapor deposition, and the thickness of the film can be accurately controlled by controlling the number of reaction cycles. Optionally, 30-60 process cycles are repeated to achieve the desired film thickness.

[0059] In an optional embodiment, the semiconductor thin film forming method further includes: step S8, chemical mechanical grinding and etching the semiconductor substrate. Optionally, chemical mechanical grinding and etching are performed to make the semiconductor thin film flat or remove redundant parts.

[0060] 4(A) to 4(E) are schematic diagrams of a thin film forming process of a semiconductor thin film forming method according to an embodiment of the present application.

[0061] FIG. 4(A) is a schematic diagram of a memory bit line of a semiconductor structure without forming a sidewall film.

[0062] FIG. 4(B) is a schematic diagram of a memory bit line of the semiconductor structure after the first deposition layer is formed in FIG. 4(A),

[0063] FIG. 4(C) is a schematic diagram of a memory bit line of the semiconductor structure after the second deposition layer is formed in FIG. 4(B),

[0064] Figure 4(D) is a schematic diagram of the semiconductor structure memory bit line after chemical mechanical grinding and etching in Figure 4(C). Figures 4(A) to 4(D) schematically show the structural changes during the formation of the semiconductor structure memory bit line.

[0065] In some embodiments, the semiconductor substrate includes a memory bit line, a first deposition layer and a second deposition layer are formed on the sidewall of the memory bit line, the first deposition layer is a stop layer for chemical mechanical polishing, and the second deposition layer is formed by alternating first thin films and second thin films. Referring to FIG4(D), the bit line insulating layer 1, the bit line intermediate layer 2 and the bit line conductive layer 3 constitute a memory bit line in the semiconductor substrate structure, and the first deposition layer 4 and the second deposition layer 7 are deposited on the sidewall of the memory bit line.

[0066] In some embodiments, the first deposition layer 4 is deposited by ALD or PEALD.

[0067] FIG. 4(E) is a partial enlarged view of FIG. 4(D) . Referring to FIG. 4(E) , the second deposition layer 7 is formed by alternating first thin films 71 and second thin films 72 .

[0068] In some embodiments, after the first deposition layer 4 is formed, steps S1 to S7 are repeated until the ratio of the thickness of the first deposition layer 4 to the second deposition layer 7 is 1.5:1 to 3:1. For example, by repeating the steps N times, N first thin films 71 and N second thin films 72 are formed. It should be noted that steps S1-S4 are used to form the first thin film 71, and step S5 is used to form the second thin film 72. Therefore, in the process of repeating steps S1 to S7, the first thin film 71 and the second thin film 72 are alternately formed.

[0069] In some embodiments, the first film 71 is silicon oxynitride SiON, which is an intermediate phase between silicon nitride and silicon dioxide, and can effectively reduce the parasitic capacitance of the interface between silicon nitride and silicon dioxide, and alleviate the technical problem of poor contact between silicon nitride and silicon dioxide; thereafter, the second film 72 is deposited by reacting a plasma containing oxygen ions with a precursor adsorbed on a semiconductor substrate, thereby achieving the deposition of the first film 71 and the second film 72 in the same process.

[0070] Figure 5 This is a semiconductor thin film forming method according to an embodiment of the present application. 2 With N 2 Schematic diagram of the effect of gas flow ratio on parasitic capacitance of semiconductor devices.

[0071] Different O 2 With N 2 If the ratio of the gas flow rate is different, the ratio of the two elements in the plasma containing oxygen ions and nitrogen ions is different, and the ratio of oxygen ions and nitrogen ions in the first film is also different, and the parasitic capacitance generated on the semiconductor device is also different. Optionally, the first film is silicon oxynitride SiNO and the second film is silicon dioxide SiO 2 When, refer to Figure 5 And the following table, when O 2 With N 2 The gas flow ratio is 1:9, and the parasitic capacitance generated on the semiconductor device is minimal. At this time, the sum of the thicknesses of the first film and the second film is 7.51 nm, and the film contains 27% oxygen and 39% nitrogen.

[0072]

[0073]

[0074] Figure 6This is a schematic diagram of the effect of the thickness ratio of the first deposition layer and the second deposition layer on the parasitic capacitance of a semiconductor device in a semiconductor thin film formation method according to an embodiment of the present application.

[0075] In some embodiments, steps S1 to S7 are repeated until the thickness ratio of the first deposition layer to the second deposition layer is 1.5:1 to 3:1. Figure 6 As shown, when the ratio of the thickness of the first deposition layer to the second deposition layer is 1.5:1 to 3:1, the parasitic capacitance of the semiconductor device is minimum. It should be noted that the thickness of the first deposition layer remains unchanged, and steps S1 to S7 are repeated to change the thickness of the second deposition layer, thereby achieving control of the ratio of the thickness of the first deposition layer to the second deposition layer.

[0076] In some embodiments, the first deposited layer is composed of Si 3 N 4 Deposition. 3 N 4 It is a super-hard material that has lubricity and is wear-resistant, making it suitable as a barrier layer and a grinding stop layer for CMP.

[0077] Figure 7 This is a schematic diagram of a semiconductor structure according to an embodiment of the present application.

[0078] like Figure 7 In the semiconductor structure shown, a first deposition layer 4 and a second deposition layer 7 are formed on a semiconductor substrate 100 . The first deposition layer 4 is a stop layer for chemical mechanical polishing, and the second deposition layer 7 is formed by alternating first thin films 71 and second thin films 72 .

[0079] In some embodiments, a ratio of the thickness of the first deposition layer 4 to the thickness of the second deposition layer 7 in the semiconductor structure is 1.5:1 to 3:1.

[0080] In some embodiments, the first deposition layer 4 of the semiconductor structure is made of Si 3 N 4 constitute.

[0081] Figure 8 It is a schematic diagram of a memory structure of an embodiment of the present application.

[0082] like Figure 8 In the memory structure shown, the bit line insulating layer 1, the bit line intermediate layer 2 and the bit line conductive layer 3 constitute the memory bit line. The first deposition layer 4 and the second deposition layer 7 are deposited on the sidewalls of the memory bit line. The first deposition layer 4 is a stop layer for chemical mechanical polishing. Figure 7 The second deposition layer 7 is formed by alternating first thin films 71 and second thin films 72 .

[0083] It should be understood that the above specific embodiments of the present application are only used to illustrate or explain the principles of the present application, and do not constitute a limitation to the present application. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present application should be included in the protection scope of the present application. In addition, the claims attached to the present application are intended to cover all changes and modifications that fall within the scope and boundaries of the attached claims, or the equivalent forms of such scope and boundaries.

Claims

1. A method for forming a semiconductor thin film, characterized in that: include: introducing a precursor into the chamber, wherein the precursor is adsorbed on the semiconductor substrate; purging the chamber to remove unadsorbed precursor; Introducing plasma containing oxygen ions and nitrogen ions into the chamber and reacting with the precursor to deposit a first film; purging the chamber to remove unreacted plasma; Introducing plasma containing oxygen ions into the chamber to react with the precursor adsorbed on the semiconductor substrate to deposit a second film; cyclically executing the above steps until the total thickness of the first film and the second film reaches a predetermined value; The semiconductor substrate comprises a memory bit line, a first deposition layer and a second deposition layer are formed on the side wall of the memory bit line, the first deposition layer is a stop layer for chemical mechanical polishing, and the second deposition layer is formed by alternating first and second films.

2. The semiconductor thin film forming method according to claim 1, characterized in that: The precursor is a compound of silicon and hydrogen.

3. The semiconductor thin film forming method according to claim 2, characterized in that: The silicon and hydrogen compound is selected from any one of tetrakis(dimethylamino)silane (TDMAS), isopropylaminosilane (DIPAS), bis(diethylamide)silane (BDEAS), bis(tert-butylamino)silane (BTBAS), or any combination thereof.

4. The semiconductor thin film forming method according to claim 1, characterized in that: In the process, the adsorption time of the precursor and the semiconductor substrate is set to 2-10 seconds.

5. The semiconductor thin film forming method according to claim 1, characterized in that: The plasma containing oxygen ions and nitrogen ions is generated by ionizing O2 and N2 or NH3 at a gas flow ratio of 1:1-1:

20.

6. The semiconductor thin film forming method according to claim 1, characterized in that: The plasma injection time is set to 1-10 seconds.

7. The semiconductor thin film forming method according to claim 1, characterized in that: During the deposition phases of the first thin film and the second thin film, the temperature of the chamber is set to 40° C. to 110° C.

8. The semiconductor thin film forming method according to claim 1, characterized in that: Also includes: The semiconductor substrate is subjected to chemical mechanical polishing and etching.

9. The semiconductor thin film forming method according to claim 1, wherein: The thickness ratio of the first deposition layer to the second deposition layer is 1.5:1 to 3:

1.

10. The semiconductor thin film forming method according to claim 1, wherein: The first deposition layer is deposited from Si3N4.

11. A semiconductor structure comprising a first thin film and a second thin film formed by the semiconductor thin film forming method according to claim 1, characterized in that: include: A first deposition layer and a second deposition layer are formed on a semiconductor substrate, wherein the first deposition layer is a stop layer for chemical mechanical polishing, and the second deposition layer is formed by alternating first thin films and second thin films.

12. The semiconductor structure according to claim 11, characterized in that: The thickness ratio of the first deposition layer to the second deposition layer is 1.5:1 to 3:

1.

13. The semiconductor structure according to claim 11, characterized in that: The first deposition layer is composed of Si3N4.

14. A memory device comprising a first thin film and a second thin film formed by the semiconductor thin film forming method according to claim 1, characterized in that: include: A first deposition layer and a second deposition layer are formed on the side wall of the memory bit line, wherein the first deposition layer is a stop layer for chemical mechanical polishing, and the second deposition layer is formed by alternating first and second films.

Citation Information

Patent Citations

  • Method of forming silicon-containing films

    CN101889331A

  • ONO structure and manufacturing method for ONO capacitor

    CN103972080A

  • Semiconductor element and forming method thereof

    CN105322013A

  • Method for fabricating semiconductor device and method for forming dielectric layer

    CN108346559A

  • Semiconductor product insulation layer structure and preparation method thereof

    CN110085550A