Aluminosilicate glass, strengthened glass and applications

By adding tin dioxide to aluminosilicate glass and adjusting the component ratio to form [SnO4] tetrahedrons, combined with ion exchange technology, the problem of traditional glass being easily broken when dropped and punctured is solved, achieving high strength and durability. The improvement of puncture performance is suitable for the protection of smart devices and automotive glass.

CN116143402BActive Publication Date: 2024-10-22QINGYUAN CSG NEW ENERGY SAVING MATERIALS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310063589.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-31
Publication Date
2024-10-22
Estimated Expiration
2043-01-31

AI Technical Summary

Technical Problem

Traditional glass is easily broken when dropped, impacted or punctured, making it difficult to meet the needs of modern smart technology and electronic products for high strength, impact resistance and puncture resistance.

Method used

By adding a specific amount of tin dioxide (SnO2) to the raw material of aluminosilicate glass, the proportion of other components is adjusted to convert the tin atoms from six-coordinated to four-coordinated to form [SnO4] tetrahedron, which enhances the The network structure of glass improves its intrinsic strength and chemical strengthening properties, and forms a dense compressive stress layer through ion exchange to improve mechanical strength and resistance to puncture by sharp objects.

Benefits of technology

Significantly improves the puncture resistance and mechanical strength of the glass, forming a strengthened glass with a surface stress value greater than 815MPa and a stress depth exceeding 38μm, effectively protecting electronic equipment and car windows from external damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004061694070000021
    Figure BDA0004061694070000021
  • Figure BDA0004061694070000061
    Figure BDA0004061694070000061
  • Figure BDA0004061694070000151
    Figure BDA0004061694070000151
Patent Text Reader

Abstract

The present application relates to the field of glass technology, in particular to aluminosilicate glass, tempered glass and applications. In terms of mass percentage of the total mass of raw materials, the raw materials of aluminosilicate glass include: 55.4% to 65.4% SiO 2 10.2%~18.2%Al 2 O 3 , 10.7% ~ 16.7% Na 2 O, 2.2% to 6.6% K 2 O, 2.9% to 6.0% MgO, 0.1% to 3.0% ZrO 2 And 0.01% to 2.0% SnO 2 ; and the content of the raw materials also satisfies the following relationship: ZrO 2 with SnO 2 The mass ratio of SiO is 1.0 to 20.0; 2 With Al 2 O 3 The sum of the mass percentage of SnO does not exceed 77.5%. 2 The ratio of other components in the raw materials is adjusted so that the network structure of the aluminosilicate glass contains [SnO 4 ] tetrahedron, due to the large field strength of tin atoms, the chemical bonds formed are more stable, thus the intrinsic strength of the product can be improved. In addition, the aluminosilicate glass obtained has good chemical strengthening properties, and a product with good mechanical strength can be obtained through subsequent strengthening treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of glass technology, in particular to aluminosilicate glass, strengthened glass and applications. Background Art

[0002] With the rapid development of the smart technology industry and the widespread adoption of digital products in recent years, touchscreen-equipped smartphones and tablets have become an indispensable part of our lives. The protective cover material on the outermost layer of the touchscreen acts as a protective shield for the touchscreen. Traditional touchscreen cover materials are primarily made of high-aluminum glass, which offers features such as impact resistance, scratch resistance, oil resistance, anti-fingerprint resistance, and enhanced light transmittance. Conventional technologies have developed high-aluminum silicate and lithium aluminum silicate glass by increasing the aluminum oxide content in the glass or adding lithium oxide, combined with one or more chemical strengthening treatments, to achieve impact resistance, scratch resistance, drop resistance, and sweat resistance. However, mobile phones and other electronic products are often accidentally dropped. Conventional screen protectors can shatter and fail upon contact with sharp objects such as stones, gravel, or concrete, causing serious damage to the electronic device.

[0003] Furthermore, when a car is driving at high speed, stones or gravel on the ground, carried by the tires and launched at high speed towards the window glass, can also cause the glass to break and fail, further endangering the safety of the occupants. Other glass, such as architectural glass and mechanical protective windows, can also break and fail when impacted by foreign objects.

[0004] Therefore, how to improve the puncture resistance and strength of glass has become an urgent problem to be solved. Summary of the Invention

[0005] Based on this, the present application provides an aluminosilicate glass, tempered glass and applications. The aluminosilicate glass has good chemical strengthening properties and strength, and the tempered glass obtained after the strengthening treatment has good puncture resistance and mechanical strength.

[0006] In a first aspect, the present application provides an aluminosilicate glass. The raw materials of the aluminosilicate glass include, in terms of percentage by mass of the total mass of the raw materials:

[0007]

[0008] And the content of the raw materials also satisfies the following relationship:

[0009] The mass ratio of ZrO2 to SnO2 is 1.0 to 20.0;

[0010] The sum of the mass percentages of SiO2 and Al2O3 shall not exceed 77.5%.

[0011] By adding a certain amount of SnO₂ to the raw materials and adjusting the ratios of the other raw materials, the resulting aluminosilicate glass network structure contains [SnO₄] tetrahedra. Due to the strong field strength of tin atoms, the chemical bonds formed are more stable, thereby improving the intrinsic strength of the product. In addition, the resulting aluminosilicate glass has excellent chemical strengthening properties, and subsequent strengthening treatments can produce products with excellent mechanical strength.

[0012] Furthermore, by controlling the amount of SnO2 added, the transparency of the product is ensured, preventing crystallization or phase separation problems caused by excessive SnO2 content. By adjusting the ratio of ZrO2 to SnO2 in the raw materials, the two components interact to enhance the intrinsic strength of the product. By regulating the total content of SiO2 and Al2O3 in the raw materials, the melt processing properties of aluminosilicate glass are guaranteed, thus enabling its application in large-scale industrial production.

[0013] In some embodiments, the mass percentage of Al2O3 is 14.3% to 18.2% based on the mass percentage of the total mass of the raw materials.

[0014] In some embodiments, the mass percentage of SnO2 is 0.01% to 1.2% based on the mass percentage of the total mass of the raw materials.

[0015] In some embodiments, the mass ratio of ZrO2 to SnO2 is 2.0 to 20.0.

[0016] In some embodiments, the sum of the mass percentages of SiO2 and Al2O3 is 71.0% to 76.8%.

[0017] In some embodiments, the mass percentage of Na2O is 12.2% to 16.7% based on the mass percentage of the total mass of the raw materials.

[0018] In some embodiments, the mass percentage of K2O is 3.0% to 5.6% based on the mass percentage of the total mass of the raw materials.

[0019] In some embodiments, the mass percentage of MgO is 2.9% to 5.3% based on the mass percentage of the total mass of the raw materials.

[0020] In some embodiments, the raw materials for the aluminosilicate glass further include: at least one of Li2O, B2O3, ZnO, CaO, and SrO. Optionally, the mass percentage of Li2O is 0-1.0% based on the mass percentage of the total mass of the raw materials; optionally, the mass percentage of B2O3 is 0-2.0% based on the mass percentage of the total mass of the raw materials; optionally, the mass percentage of ZnO is 0-2.0% based on the mass percentage of the total mass of the raw materials; optionally, the mass percentage of CaO is 0-2.0% based on the mass percentage of the total mass of the raw materials; optionally, the mass percentage of SrO is 0-2.0% based on the mass percentage of the total mass of the raw materials.

[0021] In a second aspect, the present application provides a tempered glass obtained by tempering the aluminosilicate glass of the first aspect. Optionally, the tempered glass is obtained by chemically tempering the aluminosilicate glass of the first aspect via ion exchange. Further optionally, the exchange melt used in the ion exchange is a potassium nitrate melt.

[0022] By strengthening the aluminosilicate glass, a dense compressive stress layer can be formed on the surface of the aluminosilicate glass, resulting in a strengthened glass with a surface stress value greater than 815MPa, a stress depth exceeding 38μm, and a sharp object penetration resistance exceeding 850N, thereby effectively protecting the protected object from damage from the external environment.

[0023] In a third aspect, the present application provides a use of the tempered glass according to the second aspect in preparing protective glass. DETAILED DESCRIPTION

[0024] In order to make the above-mentioned purposes, features and advantages of this application more obvious and easy to understand, the specific implementation methods of this application are described in detail below.

[0025] However, the present application can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.

[0026] In the description of this application, "a plurality of" means at least two, for example, two, three, etc., unless otherwise specifically defined. As used herein, "at least one" refers to any one, any two, or any two or more of the listed items. As used herein, "a certain number or more" should be understood to mean a certain number or a range greater than a certain number.

[0027] The terms "and / or", "or / and", and "and / or" used in this application have an optional scope including any one of two or more related listed items, and also include any and all combinations of the related listed items, said any and all combinations including any two related listed items, any more related listed items, or a combination of all related listed items.

[0028] Where “including,” “having,” and “comprising” are used herein, it is intended to cover a non-exclusive inclusion, and another component may be added unless a clear limiting term, such as “only,” “consisting of,” etc., is used. Unless mentioned otherwise, a term in the singular may include a plural form and is not to be construed as being one in number.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application.

[0030] Traditional automotive glass, protective windows for machinery and equipment, architectural glass, and some low-end industrial control displays, TV screens, tablet screens, and mobile phone displays still use soda-lime glass. Conventional technologies enhance the strength of soda-lime glass through physical or chemical strengthening, but these technologies still fall short of the required drop resistance, impact resistance, and sharp object puncture resistance required in practical applications. Furthermore, the protective glass for current mobile phone screens is mostly made of aluminosilicate glass or lithium aluminosilicate glass. These glasses contain up to 20% aluminum oxide (aluminum oxide) by weight, which can result in excessively high melting temperatures, excessive glass viscosity and surface tension, leading to difficulties in clarifying the glass, removing bubbles, and impeding scalable production. While traditional aluminosilicate and lithium aluminosilicate glass can significantly improve their strength and puncture resistance after single or secondary strengthening, in actual testing and application, their protection against sharp objects still falls short of application requirements, and the probability of breakage and failure during a drop remains high. Furthermore, with the rapid development of the smart technology industry and the widespread adoption of digital products, increasingly stringent requirements are being placed on glass properties such as strength, drop resistance, impact resistance, and puncture resistance.

[0031] The present applicant's research has found that the reason why the puncture resistance and strength of traditional glass are difficult to further improve is mainly because physical strengthening or chemical strengthening treatments cannot improve the internal network structure of the glass, and thus cannot improve the intrinsic strength of the glass products. The present applicant accidentally discovered that by adding a specific amount of tin dioxide to the raw materials for preparing glass and adjusting the ratio of other components, the tin dioxide and other components in the raw materials can interact synergistically, thereby causing the tin atoms to undergo a six-coordinate to four-coordinate transformation, thereby transforming the [SnO6] octahedron in the system into a [SnO4] tetrahedron. Because the tetrahedron can participate in the network structure of the glass, it can improve the intrinsic strength and chemical strengthening performance of the glass.

[0032] One embodiment of the present application provides an aluminosilicate glass. The raw materials of the aluminosilicate glass include, in terms of mass percentage of the total mass of the raw materials:

[0033]

[0034] And the content of the raw materials also satisfies the following relationship:

[0035] The mass ratio of ZrO2 to SnO2 is 1.0 to 20.0;

[0036] The sum of the mass percentages of SiO2 and Al2O3 shall not exceed 77.6%.

[0037] Aluminosilicate glass, primarily composed of SiO2 and Al2O3, exhibits excellent chemical stability, electrical insulation, mechanical strength, and a low thermal expansion coefficient. SiO2 forms the backbone of the glass network, while Al2O3 acts as an intermediate to enhance its stability. This application, based on traditional aluminosilicate glass, incorporates a specific amount of tin dioxide into the raw materials, allowing it to participate in the glass network in the form of [SnO4] tetrahedra.

[0038] SiO2 is a skeleton component that constitutes the glass network structure and can improve the mechanical strength, chemical stability and heat resistance of the glass. When the SiO2 content is too high, the melting and clarification temperature of the glass increases, and the melt viscosity of the system increases, making the glass difficult to shape. When the SiO2 content is too low, it accelerates the crystallization of the glass and the thermal expansion coefficient of the resulting glass is higher. Therefore, the SiO2 content affects the overall performance of the glass. Based on this, the SiO2 content (calculated as a percentage of the total mass of the raw materials, unless otherwise specified below, all contents are percentages by mass) is 55.4% to 65.4%. Specifically, the SiO2 content can be 55.4%, 56.4%, 56.6%, 57.4%, 57.6%, 58.3%, 58.85%, 59.5%, 60.3%, 61.1%, 61.6%, 62.4%, 62.6%, 63.1%, 63.9%, 64.1%, 65.1% or 65.4%.

[0039] Al2O3 is an intermediate in the glass network structure, participating in the formation of the glass network structure and enhancing the stability of the network structure. Al2O3 can also reduce the crystallization tendency of glass and improve the chemical stability, thermal stability, hardness and mechanical strength of glass. 3+ [AlO4] tetrahedra can be formed. Because the network structure of [AlO4] tetrahedra is larger than that of [SiO4] tetrahedra, it facilitates the migration and diffusion of free ions. Therefore, the addition of Al2O3 promotes ion exchange. However, when the Al2O3 content is too high, the viscosity and melting temperature of the system increase, which in turn makes it difficult to clarify the glass and remove bubbles, and affects the processing and post-processing properties of the glass. When the Al2O3 content is too low, ion exchange is not conducive, and the stability and mechanical strength of the resulting glass products are poor, making it difficult to meet the requirements of practical applications. Based on this, the Al2O3 content is 10.2% to 18.2% in terms of mass percentage of the total mass of the raw materials. Specifically, the Al2O3 content can be 10.2%, 11.0%, 12.2%, 13.1%, 14.2%, 15.2%, 16.2%, 17.0%, 17.7%, or 18.2%.

[0040] In a specific example, the mass percentage of Al2O3 based on the total mass of the raw material is 14.3% to 18.2%. Specifically, the Al2O3 content can be 14.3%, 14.75%, 15.7%, 16.5%, 17.7%, 18.0% or 18.2%.

[0041] In a specific example, the sum of the mass percentages of SiO2 and Al2O3 does not exceed 77.6%. When the total mass percentage of SiO2 and Al2O3 is higher than 77.6%, the melting temperature of the system exceeds 1680°C, while the melting temperature of a conventional glass melting furnace is less than 1680°C. Therefore, when the total content of SiO2 and Al2O3 is too high, it is difficult to meet the melting requirements of the glass melting furnace during the glass preparation process, and large-scale production may not be possible. In addition, if the total content of SiO2 and Al2O3 is too high, the bubbles generated during the melting process cannot be discharged in time, making it difficult to obtain homogeneous and qualified products.

[0042] In a specific example, the sum of the mass percentages of SiO2 and Al2O3 is 71.0% to 76.8%. Specifically, the sum of the mass percentages of SiO2 and Al2O3 is 71.0%, 72.1%, 72.6%, 73.6%, 73.8%, 74.3%, 74.6%, 75.1%, 75.55% or 76.8%.

[0043] Na2O can provide free oxygen, breaking Si-O-Si or Si-O-Al bonds, thereby lowering the melting temperature of the system and facilitating the clarification and homogenization of the glass. When the Na2O content is too low, it is not conducive to melting and molding. When the Na2O content is too high, the thermal expansion coefficient of the product increases, and the thermal shock resistance and thermal stability decrease. In addition, Na2O is the main component of ion exchange, and the Na2O content can affect the ion exchange process. Based on this, the Na2O content is 10.7% to 17.2% in terms of mass percentage of the total mass of the raw materials. Specifically, the Na2O content can be 10.7%, 11.2%, 12.7%, 13.7%, 14.7%, 15.3%, 16.0%, 16.7% or 17.2%.

[0044] In a specific example, the mass percentage of Na2O is 12.2% to 16.7% based on the mass percentage of the total mass of the raw materials. Specifically, the content of Na2O can be 12.2%, 13.2%, 14.0%, 15.0% or 16.7%.

[0045] K2O can form a "mixed alkali effect" in the system, that is, a small amount of K2O replaces Na2O to improve the melting properties, ion exchange rate and acid and alkali resistance of the glass. However, when the K2O content is too high, it will affect the ion exchange rate and weather resistance. Based on this, the content of K2O is 1.9% to 6.9% in terms of mass percentage of the total mass of the raw materials. Specifically, the content of K2O can be 1.9%, 2.2%, 2.3%, 3.0%, 4.2%, 4.6%, 5.0%, 5.6%, 6.6% or 6.9%.

[0046] In a specific example, the mass percentage of K2O is 3.0% to 5.6% based on the mass percentage of the total mass of the raw material. Specifically, the content of K2O may be 3.0%, 3.6%, 4.3%, 5.3% or 5.6%.

[0047] MgO is an external oxide in the glass network structure and can act as a reinforcing agent. MgO can also lower the melting point of glass, improve uniformity, increase hydrolysis resistance, and improve durability. However, the addition of MgO can adversely affect the compressive stress depth of the product. Based on this, the MgO content is 2.9% to 6.0% in terms of mass percentage of the total mass of the raw materials. Specifically, the MgO content can be 2.9%, 3.4%, 4.0%, 4.5%, 4.8%, 5.3%, 5.9%, or 6.0%.

[0048] In a specific example, the mass percentage of MgO is 2.9% to 5.3% based on the mass percentage of the total mass of the raw materials. Specifically, the MgO content can be 2.9%, 3.0%, 3.5%, 4.4%, 4.9%, 5.2% or 5.3%.

[0049] ZrO2 is a common crystal nucleating agent and can participate in the network structure of glass in the form of [ZrO4] tetrahedron and [ZrO6] octahedron, thereby improving the strain point, mechanical strength, stability and alkali resistance of the glass. However, if the ZrO2 content is too high, it will cause problems such as crystallization, difficulty in melting and excessively high molding temperature. Based on this, the content of ZrO2 is 0.1% to 3.0% in terms of mass percentage of the total mass of the raw materials. Specifically, the content of ZrO2 can be 0.1%, 0.5%, 0.6%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.5%, 1.6%, 1.7%, 1.8%, 2.0%, 2.3%, 2.5%, 2.6% or 3.0%.

[0050] SnO2 is typically used as a clarifier, typically forming [SnO6] octahedra and not incorporating into the glass network. Its primary function is to reduce the bubble content within the glass, thereby increasing the average visible light transmittance. However, the present applicant has discovered that under certain circumstances, SnO2 can participate in the glass network in the form of [SnO4] tetrahedra, interacting with ZrO2 and significantly enhancing the intrinsic strength of aluminosilicate glass. [SnO4] tetrahedra can be characterized by coordination number analysis of the product using instruments such as XRD, though the present applicant does not limit the specific testing methods. Under the raw material formulation of the present application, the increase in free oxygen and / or bridging oxygen in the system causes the tin atoms to transition from hexacoordinated to tetracoordinated, forming [SnO4] tetrahedra. Furthermore, due to the greater field strength of the tin atoms, the resulting Sn-O chemical bonds are more stable, meaning that the [SnO4] tetrahedra are more stable. Furthermore, the [SnO4] tetrahedra can participate in the glass network, thereby enhancing the intrinsic strength of the glass. It should be noted that the formation mechanism of [SnO4] tetrahedron is not limited to the above mechanism. In addition, when the product is subjected to external force impact, the [SnO4] tetrahedron can be converted into [SnO6] octahedron and precipitated from the network structure, causing the glass to deform and improve the toughness of the glass. The macroscopic manifestation is the improvement of puncture resistance and impact resistance. However, when the SnO2 content is too high, problems such as crystallization or phase separation and emulsification are prone to occur. Based on this, the content of SnO2 is 0.01% to 2.0% in terms of mass percentage of the total mass of the raw materials. Specifically, the content of SnO2 can be 0.01%, 0.02%, 0.05%, 0.11%, 0.15%, 0.65%, 0.71% or 2.0%.

[0051] In a specific example, the mass percentage of SnO2 is 0.1% to 1.6% based on the mass percentage of the total mass of the raw material. Specifically, the content of SnO2 can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5% or 1.6%.

[0052] Understandably, due to the exchange effect between ZrO2 and SnO2, the mass ratio of ZrO2 to SnO2 will affect the puncture resistance and mechanical strength of the glass. In addition, in the actual production process, the range of the mass content ratio of ZrO2 to SnO2 must be determined in combination with the meltability, clarification and mass producibility of the glass. Based on this, the mass ratio of ZrO2 to SnO2 is 1.0 to 20.0. When the above ratio is less than 1.0, the improvement of the intrinsic strength of the product is effective, it is difficult to meet the requirements of actual applications, and it may also affect the strengthening performance of the product. When the above ratio is greater than 20.0, the mechanical strength of the strengthened glass obtained by strengthening is reduced. Specifically, the mass ratio of ZrO2 to SnO2 can be 1.0, 1.1, 1.3, 1.5, 1.6, 2.0, 2.2, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0, 12.0, 13.0, 14.0, 15.0, 16.0, 17.0, 18.0, 19.0 or 20.0.

[0053] In a specific example, the mass ratio of ZrO2 to SnO2 is 2.0 to 20.0. Specifically, the above ratio can be 2.5, 2.7, 2.8, 3.3, 3.5, 3.6, 2.4, 4.7, 5.5, 10.9, 15.2 or 20.0.

[0054] By adding a certain amount of SnO2 to the raw materials, the network structure of the resulting aluminosilicate glass contains [SnO4] tetrahedrons. Due to the large field strength of tin atoms, the chemical bonds formed are relatively stable, and these tetrahedrons can participate in the network structure of the glass, thereby improving the intrinsic strength of the glass product. When the product is subjected to external force, the [SnO4] tetrahedrons can be converted into [SnO6] octahedrons and precipitated from the network structure, causing the glass to deform and improve its toughness. Macroscopically, it manifests as improved puncture resistance and impact resistance. In addition, the resulting aluminosilicate glass has good chemical strengthening properties, and can be subjected to subsequent strengthening treatment to obtain products with good mechanical strength.

[0055] Furthermore, by controlling the amount of SnO2 added, the transparency of the product is ensured, preventing crystallization or phase separation problems caused by excessive SnO2 content. By adjusting the ratio of ZrO2 to SnO2 in the raw materials, the two components interact, resulting in higher intrinsic strength in the product. By regulating the total content of SiO2 and Al2O3 in the raw materials, the melt processing properties of the aluminosilicate glass are guaranteed, thus enabling its application in large-scale industrial production.

[0056] In a specific example, the raw materials of the aluminosilicate glass further include, in terms of the mass percentage of the oxides, at least one of Li2O, B2O3, ZnO, CaO and SrO.

[0057] Li in Li2O + It has a smaller radius, so the addition of Li2O is beneficial to ion exchange, which can increase the compressive stress depth of the strengthened glass, reduce the thermal expansion coefficient, and improve the chemical stability. Li2O can also act as a flux to improve the processing performance of the system. However, when the Li2O content is too high, the hardness of the product will be reduced. In a specific example, the mass percentage of Li2O is 0 to 1.0% based on the mass percentage of the total mass of the raw materials. Specifically, the content of Li2O can be 0, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1.0%.

[0058] B2O3 can act as a flux and can reduce the viscosity of glass under high temperature conditions. At low temperatures, it can form [BO4] tetrahedrons, making the structure of the product more compact and improving the stability of the product. However, if the B2O3 content is too high, it will reduce the strain point and Young's modulus of the glass and may also affect the clarification effect of the glass. In a specific example, the mass percentage of B2O3 is 0 to 2.5% based on the mass percentage of the total mass of the raw materials. Specifically, the B2O3 content can be 0, 0.2%, 0.3%, 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 2.0% or 2.5%.

[0059] ZnO can help melt glass, improve the light transmittance of glass, and make the glass less likely to lose transparency. ZnO can also form [ZnO4] tetrahedrons, which reconnect the broken network structure, thereby improving the density and hardness of the product. However, when the content is too high, it will have an adverse effect on the compressive stress of the glass. In a specific example, the mass percentage of ZnO is 0 to 2.0% based on the mass percentage of the total mass of the raw materials. Specifically, the ZnO content can be 0, 0.5%, 1.0%, 1.5% or 2.0%.

[0060] CaO can relax the network structure formed by [SiO4] tetrahedra, improve the melting properties of glass at high temperatures, and prevent the glass from devitrifying. However, if the content is too high, it will affect the weather resistance of the glass and hinder the ion exchange process. In one specific example, the mass percentage of CaO is 0 to 2.0% based on the mass percentage of the total mass of the raw materials. Specifically, the CaO content can be 0, 0.5%, 1.0%, 1.5%, or 2.0%.

[0061] SrO acts as a flux to prevent glass from crystallizing. However, excessive SrO content can increase the density of the glass, resulting in excessive weight in the finished product. In one specific example, the SrO content is 0-2.0% by mass, based on the total mass of the raw materials. Specifically, the SrO content can be 0, 0.5%, 1.0%, 1.5%, or 2.0%.

[0062] In a specific example, the raw materials of aluminosilicate glass include, in terms of mass percentage of the total mass of the raw materials: 56.4% to 62.95% SiO2, 11.0% to 18.2% Al2O3, 12.2% to 16.7% Na2O, 3.0% to 5.6% K2O, 2.9% to 5.5% MgO, 0.1% to 2.2% ZrO2, 0.1% to 2.0% SnO2, 0 to 1.0% CaO, the mass ratio of ZrO2 to SnO2 is 1.0 to 2.7, and the sum of the mass percentages of SiO2 and Al2O3 is 71.1% to 76.6%.

[0063] In a specific example, the raw materials of aluminosilicate glass include, in terms of mass percentage of the total mass of the raw materials: 55.4% to 60.4% SiO2, 13.2% to 18.2% Al2O3, 0 to 0.2% Li2O, 13.1% to 16.7% Na2O, 2.2% to 5.6% K2O, 3.0% to 5.9% MgO, 2.3% to 2.8% ZrO2, 0.05% to 0.5% SnO2, 0 to 1.0% ZnO, the mass ratio of ZrO2 to SnO2 is 1.0 to 13.0, and the sum of the mass percentages of SiO2 and Al2O3 is 73.6% to 76.8%.

[0064] In a specific example, the raw materials of aluminosilicate glass include, in terms of mass percentage of the total mass of the raw materials: 57.4% to 65.4% SiO2, 10.2% to 17.7% Al2O3, 0 to 1.0% Li2O, 10.7% to 16.0% Na2O, 2.6% to 6.6% K2O, 2.9% to 6.0% MgO, 0.1% to 2.0% ZrO2, 0.01% to 1.1% SnO2, 0 to 2.0% ZnO, 0 to 2.0% SrO, the mass ratio of ZrO2 to SnO2 is 1.0 to 20.0, and the sum of the mass percentages of SiO2 and Al2O3 is 73.09% to 77.5%.

[0065] In a specific example, the raw materials of aluminosilicate glass include, in terms of mass percentage of the total mass of the raw materials: 55.4% to 65.4% SiO2, 14.3% to 18.2% Al2O3, 0 to 1.0% Li2O, 12.2% to 16.7% Na2O, 3.0% to 5.6% K2O, 2.9% to 5.3% MgO, 0.1% to 3.0% ZrO2, 0.01% to 1.2% SnO2, 0 to 2.0% ZnO, 0 to 2.0% CaO, 0 to 2.0% SrO, the mass ratio of ZrO2 to SnO2 is 2.0 to 20.0, and the sum of the mass percentages of SiO2 and Al2O3 is 71.0% to 76.8%.

[0066] The aluminosilicate glass of the present application can be prepared by, but is not limited to, the following method, which specifically includes the following steps:

[0067] S1, melting the raw materials to obtain glass liquid;

[0068] S2. Shape the glass liquid to prepare aluminosilicate glass.

[0069] In a specific example, in S1, the melting temperature is 1500-1650°C for 8 hours. The temperature is then lowered to 1300-1500°C and held for 2 hours. In S2, the glass blocks are prepared by pouring the molten glass into a mold at 450°C. Once the glass blocks have hardened, they are immediately transferred to an annealing furnace for 2 hours. Finally, the temperature is lowered to 140°C over 6 hours, allowed to cool naturally, and then removed for later use.

[0070] Another embodiment of the present application further provides a strengthened glass obtained by strengthening any of the above-mentioned aluminosilicate glasses. Optionally, the aluminosilicate glass is chemically strengthened by ion exchange to obtain the strengthened glass.

[0071] By strengthening the aluminosilicate glass, a dense compressive stress layer can be formed on the surface of the aluminosilicate glass, resulting in a strengthened glass with a surface stress value greater than 815MPa, a stress depth exceeding 38μm, and a sharp object penetration resistance exceeding 850N, thereby effectively protecting the protected object from damage from the external environment.

[0072] The tempered glass of the present application can be prepared by, but is not limited to, the following method, which specifically includes the following steps:

[0073] S3. Strengthening the aluminosilicate glass.

[0074] Before step S3, the glass block is cut into glass sheets of a predetermined size. Step S3 can be performed by immersing the glass sheets in a potassium nitrate melt at 390-430°C for 3-8 hours to cause ion exchange in the glass sheets, thereby achieving chemical strengthening. It should be noted that the glass involved in this application can be obtained in a conventional flat glass manufacturing process, and its manufacturing process is not limited to float forming process, overflow downdraw method, draw-up method, flat draw method, rolling method, etc.

[0075] Finally, one embodiment of the present application also provides the use of tempered glass in the preparation of cover glass. This cover glass can be used in electronic devices, windows, semiconductor devices, and other fields. Electronic devices include, but are not limited to, mobile phones, tablets, televisions, wearable devices, virtual reality (VR) devices, and augmented reality (AR) devices. The windows can be used in, but are not limited to, buildings, vehicles, and mechanical equipment. Semiconductor devices include, but are not limited to, semiconductor sensors.

[0076] In order to make the purpose and advantages of this application more clear, the following further describes this application in detail with reference to the embodiments. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit this application.

[0077] In different examples and comparative examples, the raw materials used to prepare the aluminosilicate glass and the tempering process conditions for the tempered glass vary, as shown in Tables 1-8. The specific preparation method is as follows: For Examples 1-56 and Comparative Examples 1-12, the corresponding raw materials (mass percentage) were weighed according to the proportions in Tables 1-8. After thorough mixing, the glass was melted in a platinum crucible at 1500-1650°C for 8 hours while stirring with a platinum stirring paddle. After the stirring paddle was removed, the temperature was lowered to 1300-1500°C, held for 2 hours, and homogenized. The glass was then cast into an iron mold to form an aluminosilicate glass block of approximately 80*160 mm in size. The mold was preheated to 450°C before casting. After hardening, the glass block was immediately transferred to an annealing furnace for annealing, held for 2 hours, then cooled to 140°C within 6 hours, and removed after natural cooling for use.

[0078] Aluminosilicate glass blocks were cut into 70 x 140 x 1.1 mm sheets using a Shenyang Kejing STX-1203 wire saw. These were then thinned and polished using a Shenzhen Hyde HD-640-5L double-sided grinding and polishing machine, followed by CNC edge grinding. The density of the samples was measured using a Wuxi Kesairui AKD-120A solid density and volume tester, while the thermal expansion coefficient was measured using a Netzsch DIL 402 Expedis Classic dilatometer. The softening point of the samples was measured according to the national standard GB / T 28195-2011. The test results are shown in Tables 1 to 8.

[0079] The aluminosilicate glass sheets from each example and comparative example were then chemically tempered to produce tempered glass. The tempering times and temperatures are shown in Tables 1-8. It should be noted that Tables 1-8 only provide a selection of optional tempering process parameters; those skilled in the art can select specific tempering process parameters based on actual needs. Specifically, the aluminosilicate glass sheets were immersed in a potassium nitrate melt at a predetermined tempering temperature for a predetermined tempering time, and ion exchange was performed.

[0080] The surface compressive stress CS and compressive stress depth Dol of the tempered glass were tested using the FSM6000LE stress tester from Orihara, Japan. The ultimate falling ball energy of the tempered glass was tested using the ZJ-9968 drop ball tester from Zhengjie Instruments, specifically using an 110g steel ball. The ring compression strength of the tempered glass was tested using the PT-307A universal testing machine from Puset (upper ring φ = 16mm, lower ring φ = 32mm). The maximum pressure resistance of the tempered glass to the sharp object puncture resistance was obtained using the ST-DT100 pressure tester from Sitai Instruments, using a tungsten steel indenter with φ = 0.5mm to squeeze the glass surface until it breaks. The test results are shown in Tables 1 to 8. It should be noted that in the following tables, ZrO2 / SnO2 represents the mass ratio of ZrO2 to SnO2, and SiO2+Al2O3 represents the sum of the mass percentages of SiO2 and Al2O3.

[0081] Table 1

[0082]

[0083]

[0084] Table 2

[0085]

[0086]

[0087] Table 3

[0088]

[0089]

[0090] Table 4

[0091]

[0092]

[0093] Table 5

[0094]

[0095]

[0096] Table 6

[0097]

[0098]

[0099] Table 7

[0100]

[0101]

[0102] Table 8

[0103]

[0104]

[0105] Please refer to Tables 1 to 7. Examples 1 to 56 have good mechanical strength, the falling ball strength can reach more than 1.49J, the strength can reach more than 3000N, and the sharp object puncture strength can reach more than 850N, and the appearance of the samples of Examples 1 to 56 is transparent. In some preferred embodiments, the falling ball strength can reach more than 1.80J, the strength can reach more than 4000N, and the sharp object puncture strength can reach more than 1100N, which can effectively prevent sharp objects from damaging the window glass and protect people in the car. When the above-mentioned glass is used as a screen for electronic equipment, or is used in semiconductor sensors and other fields, it can effectively protect related equipment. In addition, the samples of Examples 1 to 56 form a dense compressive stress layer on the surface, the stress value can reach more than 815MPa, and the stress depth exceeds 38μm, indicating that the samples of each example have good chemical strengthening properties.

[0106] Further, referring to Tables 1 to 5, the values ​​of ZrO2 / SnO2 in Examples 1 to 45 increase successively. Overall, the mechanical strength of the samples in the above-mentioned examples increases, indicating that when the value of ZrO2 / SnO2 is within a suitable range (e.g., 2.0 to 20.0), SnO2 can form a certain amount of [SnO4] tetrahedrons and can also interact with ZrO2, thereby improving the strength of the sample. It should be noted that the raw material components in each example as a whole affect the processing and forming properties, strengthening and strength properties of the sample. Therefore, when analyzing and comparing the performance of each example, it is necessary to consider the overall raw material formula and the synergistic effect between the various raw material components. In other words, the present application has obtained the raw material formula of the present application through a large number of experiments and comprehensive consideration of the intrinsic strength, processing properties (e.g., softening temperature) and strengthening properties of aluminosilicate glass, so that the strengthened product has good mechanical strength.

[0107] Please refer to Table 7. Comparative Example 1 does not contain SnO2, so it cannot form [SnO4] tetrahedrons that participate in the glass network structure. The glass structure has the inherent characteristics of traditional brittle materials, and its falling ball strength, ring crush strength and sharp object puncture strength are greatly reduced. In Comparative Example 2, the SnO2 content exceeds 2wt%. When the alkali metal / alkaline earth metal content is relatively high, SnO2 participates in the glass network in the form of [SnO4] tetrahedrons and [SnO6] octahedrons, and as the SnO2 content increases, the [SnO6] octahedron structure occupies the majority. Since the [SnO6] octahedron cannot participate in the glass network structure and can only enter the structural gap, the intrinsic strength is reduced. More importantly, due to the high field strength of the [SnO6] octahedron, aggregation is likely to occur, increasing the tendency of crystallization, resulting in a small amount of phase separation of the glass, reducing the optical transmittance, and the appearance is semi-transparent.

[0108] In Comparative Example 3, the ZrO2 / SnO2 ratio is less than 1, and in Comparative Example 4, the ZrO2 / SnO2 ratio is greater than 20, and the sharp object puncture strength is significantly reduced. In addition, the strengthening stress depth Do1, the ball drop strength, and the ring crush strength in Comparative Example 3 are also significantly reduced.

[0109] In Comparative Example 5, the MgO content was reduced to 1.5wt%, significantly reducing its role in modifying the glass network structure. This resulted in a loosening of the glass structure and a significant decrease in its surface compressive stress, directly impacting the strength properties of the strengthened glass, particularly its ring crush and sharp object puncture resistance. In Comparative Example 6, the MgO content was increased to 7.8wt%. More MgO filled the interstices of the glass structure. Due to its low molecular weight, MgO blocked ion exchange channels, reducing ion exchange capacity and lowering its strengthening stress depth, Dol, directly impacting the product's ball drop, ring crush, and sharp object puncture resistance properties.

[0110] Please refer to Table 8. In Comparative Example 7, the K2O content was reduced to 2.0 wt%, which reduced the channels for K ion exchange, lowered the K / Na ion exchange efficiency, and severely reduced the ion exchange capacity. The strengthening stress depth Dol was reduced, which directly affected the ball drop, ring crush, and sharp object puncture resistance of the tempered glass. In Comparative Example 8, the K2O content was increased to 8.2 wt%. Due to the excessively high total alkali metal content, the thermal expansion coefficient exceeded 115*10 -7 1 / °C, exacerbating thermal expansion coefficient mismatch problems during subsequent thermal processing (such as hot bending, physical strengthening, and bonding). Furthermore, excessive alkali metals provide excess free oxygen, which has a strong bond-breaking ability, severely damaging the glass network structure and significantly reducing the puncture resistance of the product.

[0111] The Al2O3 content in Comparative Example 9 was reduced to 9wt%, and its chemical strengthening ability was significantly reduced, which was manifested in the reduction of surface compressive stress and compressive stress depth Dol, affecting the falling ball, ring pressure and sharp object puncture resistance of the tempered glass. The Al2O3 content in Comparative Example 10 was increased to 19.2wt%, and the glass modifier component was less, and the melting temperature and molding difficulty increased, even exceeding the temperature of conventional glass production process. In addition, the softening point also increased significantly, exceeding 840°C. Usually, automotive glass, mobile phone cover glass and some architectural glass require physical tempering, hot bending and other processes. The general heat treatment temperature does not exceed 820°C. Therefore, the sample of Comparative Example 10 is not suitable for conventional production processes and is not suitable for mass production.

[0112] In Comparative Example 11, the Na2O content was reduced to 9.9wt%, resulting in a decrease in glass modifier components and a significant increase in melting temperature, exceeding the temperature of conventional glass production processes. Furthermore, the softening point increased to 848°C, making it unsuitable for conventional production processes and unsuitable for mass production. In Comparative Example 12, the Na2O content was increased to 17.3%, and the thermal expansion coefficient increased to 115.2*10 -7 1 / ℃, which aggravates the mismatch of thermal expansion coefficient caused by subsequent thermal processing (such as hot bending, physical strengthening and bonding) and reduces the puncture resistance.

[0113] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0114] The above-described embodiments merely represent several implementation methods of the present application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that a person of ordinary skill in the art may make various modifications and improvements without departing from the spirit of the present application, all of which fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims, and the specification may be used to interpret the content of the claims.

Claims

1. An aluminosilicate glass, It is characterized in that Calculated by mass percentage of the total mass of raw materials, the aluminosilicate glass is composed of the following raw materials: Not. 2 56.4%~59.4%, <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 16.2%~18.2% So 2 14.7%~16.7%、 K 2 2.2%~4.3%, MgO 3.0%~5.2%, ZrO 2 0.2%~2.3%、 SnO 2 0.1%~1.2%、 Li 2 0%~1.0%, B 2 O 3 0.1%~2.5%、 ZnO 0~2.0%, CaO 0~2.0%, and SrO 0~2.0%; And the content of the raw materials also satisfies the following relationship: The ZrO 2 With the SnO 2 The mass ratio is 4.5~19; The SiO 2 With the Al 2 O 3 The sum of the mass percentages shall not exceed 77.6%.

2. The aluminosilicate glass according to claim 1, It is characterized in that The SiO 2 With the Al 2 O 3 The sum of the mass percentages is 72.6%~76.8%.

3. The aluminosilicate glass according to claim 1, It is characterized in that In terms of mass percentage of the total mass of the raw materials, the Li 2 The mass percentage of O is 0.2%~1.0%.

4. The aluminosilicate glass according to claim 1, It is characterized in that In terms of mass percentage of the total mass of the raw materials, the B 2 O 3 The mass percentage is 0.1%~1.2%.

5. The aluminosilicate glass according to claim 1, It is characterized in that Calculated by mass percentage of the total mass of the raw materials, the mass percentage of CaO is 0.5% to 2.0%.

6. A tempered glass, It is characterized in that The method is obtained by strengthening the aluminosilicate glass according to any one of claims 1 to 5.

7. The tempered glass according to claim 6, It is characterized in that The tempered glass is obtained by chemically strengthening the aluminosilicate glass according to any one of claims 1 to 5 by ion exchange.

8. The tempered glass according to claim 7, It is characterized in that The exchange molten liquid used in the ion exchange is a potassium nitrate molten liquid.

9. Use of the tempered glass according to any one of claims 6 to 8 in the preparation of protective glass.