Method for fabrication of micro-channels inside soda silicate glasses by ultrafast laser lithography

The method employs ultrafast laser lithography and selective chemical etching to create high-aspect-ratio, fully-open micro-channels within soda silicate glasses, addressing the challenge of surface damage and curved geometry limitations, achieving precise and reproducible micro-channel fabrication.

WO2024228684A1PCT designated stage expired Publication Date: 2024-11-07BILKENT UNIVERSITESI ULUSAL NANOTEKNOLOJI ARASTIRMA MERKEZI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/TR2023/050438
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-07

Smart Images

  • Figure TR2023050438_07112024_PF_FP_ABST
    Figure TR2023050438_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention discloses a method for making fully-opened micro-channels of desired position and depth to be embedded in soda silicate glasses using an ultrafast laser-writing process and selective chemical etching. The method of the present invention is applicable to soda-lime silicate glass compositions with low (>1%) aluminum oxide content, to soda-lime silicate glass compositions with relatively high (>3%) aluminum oxide content, and to soda silicate glass with up to 10 6% aluminum oxide content.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD FOR FABRICATION OF MICRO-CHANNELS INSIDE SODA SILICATE GLASSES BY ULTRAFAST LASER LITHOGRAPHY

[0002] Technical Field

[0003] The present invention relates to a method that enables the fabrication of fully-open micro-channels at a desired position and depth inside soda silicate glasses, as embedded (buried) inside the glass and without damaging the glass surface, by means of laser writing and selective chemical etching.

[0004] Prior Art

[0005] Soda silicate glasses account for around 90% of global glass production and are the most widespread glass family, finding applications in a wide range of markets, such as construction, transportation, photovoltaics, consumer electronics, and biomedical instruments. Femtosecond (fs) lasers have unique advantages, including minimal collateral damage around the interaction area, enabling localized modifications at the nano- / micro-scale. These lead to controlled 3D fabrication with numerous functionalities in transparent materials, such as the formation of optical gratings inside a laser-written soda-lime glass (Li, Yan, et al. "Holographic fabrication of multiple layers of grating inside soda-lime glass with femtosecond laser pulses." Appl. Phys. 80.9 (2002): 1508-1510.), fabrication of micropillar arrays on the material surface (Chang, Tien-Li, et al, "Ultrafast laser ablation of soda-lime glass for fabricating microfluidic pillar array channels." Microelectron. Eng. 158 (2016): 95-101.), as well as the creation of capillary channels on the surface (Aymerich, M., et al. "Soda-lime glass as biocompatible material to fabricate capillary -model devices by laser technologies." Opt. Mat. Express 12.5 (2022): 1790-1806.). Despite the ubiquitous use of soda silicate glasses in multiple industries, there is no proven method based on ultrafast laser lithography to create micro-channels inside soda silicate glass, and further position them in a manner that these channels do not cut the top / bottom surfaces of glass. In particular, laser- fabrication of fully-opened multilayered or curved micro-channels embedded (buried) in soda silicate glasses has not been reported in the literature.

[0006] Non-diffracting ultrashort pulses in the filament regime directly produces taper-free micro / nano-channels inside borosilicate glass but longer channels necessitate higher pulse energies (Bhuyan, M.K., et al. "High aspect ratio nanochannel machining using single shot femtosecond Bessel beams." Appl. Phys. Lett. 97.8 (2010): 081102.) (Bhuyan, M. K., et al. "High aspect ratio taper-free microchannel fabrication using femtosecond Bessel beams." Opt. Express 18.2 (2010): 566-574.) (Mitra, S., et al. "Millijoule femtosecond micro-Bessel beams for ultra-high aspect ratio machining." Appl. Opt. 54.24 (2015): 7358-7365.). Since the optical filaments are aligned with the optical axis of the focusing optics the entrance and exit surfaces on the glass sample are damaged so that the ablation debris can be removed. In this approach, unlike the present invention, micro-channels of arbitrarily curved geometry is not possible.

[0007] Patent US 2010 / 0038825 Al describes a method for creating micro-channels in optically transparent materials using ultrafast lasers but requires the presence of two materials with different ablation thresholds. Patent No. US 2018 / 0340262 Al describes a method for creating micro-channels through the thickness of the plate in silicate glasses. The method is based on acidic etching, further, ultrasonication is used during the etching process, and the final produced channels elongate between the top and bottom surfaces of the glass, that is, between the laser entrance and exit surfaces, unlike in this invention, where the laser entrance and exit surfaces (i.e., top and bottom surfaces) are unaltered at the end of all involved steps. In addition, unlike in this invention, curved channel production is not possible.

[0008] A work similar to the present invention is described in US Patent No. 11275215 B2. Therein, various optical micro-elements are fabricated as structural elements in fused silica, using HF solution as the main abrasive and a 1030 nm wavelength laser with a pulse duration of 350 fs as the light source. Another method similar to the present invention has been used to create micro-channels in fused silica (Casamenti, Enrico, et al. "Few pulses femtosecond laser exposure for high-efficiency 3D glass micromachining." Opt. Express 29.22 (2021): 35054-35066.). In that study, a femtosecond laser with a wavelength of 1030 nm was used in combination with three alternative wet etching solutions, two different alkaline-based etching solutions, and one acidic solution. In the present invention, NaOH-based etching is preceded by a pre-etching step with HF. Unlike fused silica, the soda silicate glasses of the present invention contain components such as Na2O, CaO, MgO, and AI2O3 which act as network modifiers and intermediate oxides and interrupt the tetrahedral SiCh network, and the glass is chemically differentiated from fused silica. The presence of such oxides in the glass structure is known to directly alter laser ablation thresholds (Lee, Hyeon-Min, et al. "Effect of the chemical composition on the ablation characteristics of glass substrates in femtosecond laser machining." Int. J. ofPrecis. 18.11 (2017): 1495-1499.). In addition, it has been found that the etching selectivity in the formation of structural elements is also lower in glasses with boron oxide content, as the base etching rate in the non-laser-exposed regions is higher than in pure fused silica (Bischof, David, et al. "Laser-assisted etching of borosilicate glass in potassium hydroxide." Opt. Mater. Express 11.4 (2021): 1185- 1195.). In the present invention, the wavelength is chosen (800 nm), which is shorter than the aforementioned studies, enabling the reduction of wasted power due to the absorption band, which is centered around 1100 nm originating from the iron content in soda silicate glasses.

[0009] The work closest to the present scope of the invention suggests that micro-channels can be created by laser etching and chemical etching (20 min with HF and 5 min with NaOH solution at a molarity concentration of 2 mol / L), but does not mention the dimensions of the opening port region where the channels open, the length of the channels after etching, or whether these channels are partially or fully opened (Fiorin, Rodrigo, et al. "Manufacturing of micro-channels in soda-lime glass by femtosecond laser and chemical etching." 2013 SBMO / IEEE MTT-S International Microwave & Optoelectronics Conference (IMOC). Rio de Janeiro, Brazil, 2013. 1-3.). The authors use HF as the main etchant and use NaOH solution to stop the HF-based reaction. In the context of the present invention, HF is used in the pre- etching step and NaOH acts as the main etchant. In addition, unlike in this invention, curved channel production is not possible.

[0010] Brief Description of the Invention

[0011] One object of the present invention is to fabricate high-aspect-ratio, fully-open micro-channels in soda silicate glasses by laser writing and selective chemical etching, created at the desired positions and depths, and embedded inside the glass without damaging any surfaces of the glass material (except opening ports at the end of the microchannels).

[0012] The second object of the present invention is to produce high-aspect-ratio fully- open micro-channel arrays in soda silicate glasses, located at the desired position and depth, and embedded inside soda silicate glass without damaging any surfaces of the material (except opening ports at the end of microchannels), by laser writing and selective chemical etching.

[0013] Another aim of the present invention is to fabricate multi-layered high-aspect-ratio fully-open micro-channel arrays inside soda silicate glasses in a controlled, fast, and reproducible manner, by laser writing and selective chemical etching, and without damaging any surfaces of the glass material (except opening ports at the end of microchannels).

[0014] Detailed Description of the Invention

[0015] The "Method For Fabrication Of Micro-Channels Inside Soda Silicate Glasses By Ultrafast Laser Lithography" which is realized to achieve the objects of the present invention is shown in the attached figures;

[0016] Figure 1. A flowchart of the inventive method.

[0017] Figure 2. The general configuration of linear and curved micro-channels inside the glass. The dimensions of the micro-channel are shown as di, d2 and ds indicating the length of the small principal axis of the opening port, the length of the large principal axis of the opening port and the depth of the micro-channel, respectively. The direction of the longitudinal depth of the micro-channel is always in the direction of the x coordinate in the global coordinate system.

[0018] Figure 3. (a) Optical microscope image of the x-y surface and (b) scanning electron microscope (SEM) image of the y-z surface of a fully-open micro-channel measuring 10 pm x 15 pm x 500 pm, embedded inside soda-lime silicate glass.

[0019] Figure 4. (a) Optical microscope image of the x-y surface and (b) scanning electron microscope (SEM) image of the y-z surface of a series of fully-open micro-channel array, each with dimensions of 10 pm x 15 pm x 500 pm and embedded inside soda-lime silicate glass.

[0020] Figure 5. Optical microscopy image of (a) x-y surface and scanning electron microscopy (SEM) image of (b) y-z surface of a multi-layer channel array, consisting of fully-open micro-channels embedded in soda-lime silicate glass. The dimensions of individual micro-channels are 20 pm x 30 pm x 500 pm.

[0021] Figure 6. Optical microscope image of (a) x-y surface and (b) scanning electron microscope (SEM) image of y-z surface of a fully-open micro-channel embedded in soda silicate glass with high aluminum oxide content. The channel dimensions are 24 pm x 25 pm x 1 mm.

[0022] Figure 7. Optical microscope image of the (a) x-y surface (b) scanning electron microscope (SEM) image of the y-z surface of a series of fully-open micro-channels embedded in soda silicate glass with high aluminum oxide content. Each channel has dimensions of 24 pm x 25 pm x 1 mm.

[0023] Figure 8. Optical microscopy image of (a) x-y surface (b) scanning electron microscopy (SEM) image of y-z surface of a multilayer channel array, consisting of fully-open micro-channels embedded in soda silicate glass with high aluminum oxide content. Each micro-channel has dimensions of 24 pm x 25 pm x 1 mm Figure 9. (b) (d) Optical microscope images from the x-y planes and (a), (c), scanning electron microscope (SEM) images from the y-z cross-sections of meshtype architecture, fully-open micro-channels fabricated inside soda silicate glass with high aluminum oxide content. The dimensions of micro-channels are (a, b) port opening of 15 pm x 17 pm with 20 pm period, (c, d) port opening of 25 pm x 25 pm with 100 pm period. The lattice arrays were formed inside a cube-shaped soda-silicate glass with high aluminum oxide content (1 mm x 1 mm x 1 mm).

[0024] Figure 10. (a) Optical microscope images from the x-y plane, and (b) SEM images from the y-z cross-section of a series of U-shaped fully-open micro-channels inside soda silicate glass with high aluminum oxide content. The port openings are 48 pm x 51 pm, and channel length along x axis is 550 pm. The separation between U- shaped channels inside soda-silicate glass with high aluminum oxide content is 150 pm. The radius of the circular section is 185 pm.

[0025] 100. Method

[0026] The inventive method (100), which enables fully-open micro-channels to be produced in soda silicate glass containing up to 6% aluminum oxide at the desired position and depth, embedded inside the glass and without damaging the front and rear glass surfaces by laser writing and selective chemical etching;

[0027] - obtaining a laser beam from a light source (101),

[0028] - adjusting the power of the light transmitted from the light source (102),

[0029] - adjusting the beam diameter and transmitting it to the focusing lens (103),

[0030] - obtaining modifications embedded in the glass by positioning the beam from the focusing lens into the glass and adjusting the scanning direction and speed (104),

[0031] - splitting / cutting of laser etched glass to obtain a pristine and uncontaminated interface prior to chemical etching (105),

[0032] - using a recipe for selective chemical pre-etching of high-aspect-ratio microchannels in glass (106) and

[0033] - using a recipe for selective chemical etching of high-aspect-ratio micro-channels in glass (107). In the step of obtaining a laser beam from a light source (101) of the present invention (100) specification, the light source used is an ultrafast laser with Gaussian pulses with a pulse length of less than a picosecond and a pulse repetition frequency of less than 100 kHz. The light source used has a pulse energy of at least 700 nJ. The interaction of femtosecond lasers with materials differs from systems with pulse lengths of picoseconds and above due to the use of pulses shorter than the electron-phonon scattering time scale and triggered by nonlinear absorption of photons with energies less than the electronic band gap of the material. This enables material modification in optically transparent materials in very small volumes around the focal area of the beam. Another fundamental factor determining the laser-material interaction regime is the pulse repetition rate, which is the rate at which heat is radiated into the material, and there are two distinct regions, sub-MHz and above MHz. In sub-MHz applications, material modification is based on the interaction of single pulses with the material, and since there is no heat build-up, the volume being modified is directly determined by the focusing parameters of the laser (spot diameter and depth of field). In a preferred embodiment of the invention, the laser used is an ultrafast pulsed laser with a pulse length of less than a picosecond and a pulse repetition frequency of less than 100 kHz. In a more preferred embodiment of the invention, the laser beam used has a pulse length of 150 femtoseconds and a pulse repetition frequency of 1 kHz. In a preferred embodiment of the invention, the wavelength of the laser beam was selected to be in the 300 nm to 5 pm range where soda silicate glasses are transparent. This allows processing within the volume of the material without undesirable surface absorption effects. In a more preferred embodiment of the invention, the wavelength of the laser beam can be adjusted so that it does not directly overlap with the absorption band centered at ~1100 nm; it was chosen as 800 nm so as not to directly interfere with it.

[0034] In the step of adjusting the power of the light transmitted from the light source (102) of the inventive method (100), the power of the light transmitted from the light source is controlled using a neutral density filter or any other power regulating component. The power controller allows the laser pulse energy to be varied for a constant pulse width and repetition rate.

[0035] In the step of adjusting the beam diameter and transmitting it to the focusing lens (103) of the inventive method (100), a telescope system comprising two lenses or a beam expander is used for adjusting the beam diameter, from which the beam is transmitted to the focusing lens. A microscope objective lens, an aspherical lens with a high numerical aperture (NA), or other focusing optics is used for final focusing in laser writing without masking and molding.

[0036] In the step of obtaining modifications embedded in the glass by positioning the beam from the focusing lens into the glass and adjusting the scanning direction and speed (104) of the inventive method (100), the laser beam is focused and guided into a glass sample placed on a motorized table and then laser writing is started. The NA parameter of the lenses (focusing lens) used to process the materials is decisive, and at low NA values, nonlinear effects such as self-focusing and super- continuous light generation are observed and control over the processing can be reduced. At higher NA values, the structural modification created becomes spherically symmetric, an effect that is preferable in micro-channel applications. A preferred embodiment of the invention uses a lens with an NA of at least 0.3. In a more preferred embodiment of the invention, an aspherical lens with f = 4.5 mm and NA = 0.55 focuses the beam onto a glass sample. The glass sample is moved by a motorized table in accordance with the incoming laser direction with speed and acceleration control. In silicate glasses, the process of writing into the silicate glass begins with vertical or longitudinal laser scanning according to the laser propagation direction. The size of the structural elements produced is controlled by the appropriate choice of polarization, scanning speed and direction, and power. The high level of control over the depth and position of the micro-channels within the glass sample makes it possible to arrange these micro-channels within the glass by single-line, mesh type arrays, multi-layered mesh type arrays or various curved architectures. In the preferred application of the technique, linear polarization perpendicular to the scanning direction is chosen. With the start of laser writing, two-dimensional-(2D)-constrained sub-surface modifications are obtained inside the glass sample. In the step obtaining modifications embedded in the glass by positioning the beam from the focusing lens into the glass and adjusting the scanning direction and speed (104) of the inventive method (100), in the preferred embodiment, the writing process inside the glass is carried out perpendicular to the direction of propagation of the laser beam. The size of the obtained elements can be controlled depending on the scanning speed (0.1-1 mm / s), scanning direction, laser power, and polarization of the laser beam. The pulse energy value used in the preferred embodiment of the invention was chosen to be >3 pj for the soda lime silicate glass used in the first example and > 700 nJ for the soda silicate glass with high aluminum oxide content used in the second example, in order to enable chemical etching in the next step of the writing process. The dominant parameter in the creation of micro-channels is the energy per unit area, and the total energy delivered into the material can be controlled by varying the laser power or scanning speed. In the preferred embodiment of the invention, a configuration with linear polarization and polarization direction in the scanning direction is preferred, but laser beams with circular and elliptical polarization can also produce structural changes in the material.

[0037] In the step splitting / cutting of laser etched glass to obtain a pristine and uncontaminated interface prior to chemical etching (105) of the method of the invention (100), the samples are cut so that the laser-exposed regions can be accessed by the etchant. The splitting / cutting step can be performed by diamondbased cutting, CO2 laser notch-less cutting, filamentation-based cutting, laser ablation-based cutting, or any variation thereof.

[0038] In the step using a recipe for selective chemical pre-etching of high-aspect-ratio micro-channels in glass (106) of the inventive method (100), HF solution in the molarity range of 1.5-5 mol / L is used to pre-etch the laser-treated areas. The preetching step is important for the reproducible and complete opening of the microchannels with target dimensions. In the preferred embodiment of the invention, the molarity of the HF pre-etching solution is set to 2.5 mol / L. The molarity of the HF is critical for the efficient opening of the micro-channels in the next and main etching step, and to avoid the formation of a radius structure at the edges of the micro-channel opening port area. It is known that the etching selectivity of HF increases with decreasing exposure time in fused silica glasses. A similar effect was observed in the soda silicate glasses studied in the present invention. The preetching time is described in the present invention as not exceeding 120 s and not shorter than 30 s. In case of a pre-etching time longer than 120 s, the opening port area of the micro-channels expands, and a larger channel cross-section is formed compared to the middle part of the micro-channel. In the preferred embodiment of the invention, this time is set in the range of 60-90 s.

[0039] In the step using a recipe for selective chemical etching of high-aspect-ratio microchannels in glass (107) of the inventive method (100), an aqueous NaOH solution with a molarity concentration of 7 to 12 mol / L and a temperature of at least 60°C is used as the main abrasive. It has been reported that increasing alkalinity and temperature in silico-alkali solutions accelerate the dissolution of silica. In addition, the presence of calcium, which is also present in the structure of soda lime silicate glasses, plays a decisive role in the formation of reaction products. The temperature and molarity concentration of the etching solution is determined by balancing an acceptable etch rate with high etch selectivity. In a more preferred embodiment of the invention, the concentration of the NaOH solution used for etching is set to 10 mol / L and the solution temperature is set to 90°C. In the preferred embodiment of the invention, the etching time is set to at least 1 hour to obtain a high aspect ratio. In a further preferred embodiment of the invention, the etching time is set to 6 hours.

[0040] With the method (100) according to the invention, it is possible to produce microchannels with high reproducibility and high-aspect-ratio in soda lime silicate glass containing 72.2% SiCh, 13.7% Na2O, 8.4% CaO, and 0.9% AI2O3. In this example, micro-channels with a structure size of 3 * 8 pm to 10 * 15 pm and a length of 500 pm were processed in a controlled and reproducible manner in the desired location and depth inside the soda lime silicate glass without damaging the front and back surface of the glass. The high degree of control over the depth and position of the micro-channels produced inside the glass allows them to be formed in different architectures, such as single channels (Figure 3), arrays (Figure 4), or multilayer patterns consisting of 2D arrays (Figure 5). Fully opened micro-channel arrays and multilayer micro-channel arrays formed in soda-lime silicate glass are shown in Figure 4 (a) and (b) and Figure 5 (a) and (b) respectively.

[0041] In the second example, soda silicate glass with a high aluminum oxide content of 64.9% SiCh, 16.3% Na20, 1.1% CaO, and 5.7% AI2O3 was used, which enabled the fabrication of micro-channels with high reproducibility and high length-to-width ratio. In this example, micro-channels with a structure size of 6 * 9 pm to 25 x 25 pm and a length of 1 mm were processed in a controlled and reproducible manner in the desired location and depth inside the soda silicate glass with high aluminum oxide content, without damaging the front and back surface of the glass. The high degree of control over the depth and position of the micro-channels produced inside the glass allows them to be formed in different architectures, such as single channels (Figure 6), arrays (Figure 7), multilayer patterns consisting of 2-D arrays (Figure 8) or lattice / mesh type arrays (Figure 9), which can be obtained with controllable pitch. Scanning electron microscope (SEM) and optical microscope images of the desired pitch interval patterns formed in soda silicate glass with high aluminum oxide content are shown in Figures 9 (a) and (c) and Figures 9 (b) and (d), respectively. In addition, it is possible to create curved microchannels buried inside the soda silicate glass as shown in Figure 10.

[0042] Around these basic concepts, it is possible to develop a wide variety of applications for the invention's subject matter, "Method for fabrication of micro-channels inside soda silicate glasses by ultrafast laser lithography (100)", and the invention cannot be limited to the examples described herein, but is essentially as outlined in the claims.

Claims

CLAIMS1. The inventive method for fabricating fully-open micro-channels to be produced in soda silicate glass containing up to 6% aluminum oxide at the desired position and depth, embedded inside the glass and without damaging the front and rear glass surfaces by laser writing and selective chemical etching characterized by the steps;- obtaining a laser beam from a light source (101),- adjusting the power of the light transmitted from the light source (102),- adjusting the beam diameter and transmitting it to the focusing lens (103),- obtaining modifications embedded in the glass by positioning the beam from the focusing lens into the glass and adjusting the scanning direction and speed (104),- splitting / cutting of laser etched glass to obtain a pristine and uncontaminated interface prior to chemical etching (105),- using a recipe for selective chemical pre-etching of high-aspect-ratio micro-channels in glass (106) and- using a recipe for selective chemical etching of high-aspect-ratio microchannels in glass (107).

2. A method as in claim 1 (100), characterized in the step (101) of obtaining a laser beam from a light source, wherein the light source used is an ultrafast laser having Gaussian pulses with a pulse length of less than a picosecond and a pulse repetition frequency of less than 100 kHz.

3. A method (100) as in claim 2 or 3, characterized in the step (101) of obtaining a laser beam from a light source, wherein the light source used has a pulse energy of at least 700 nJ.

4. A method (100) as in claim 3, characterized in step (101) of obtaining a laser beam from a light source, such that the beam is obtained by the light source at a wavelength in the wavelength range 300 nm - 5 pm where the silicate glasses are transparent and at a wavelength that does not overlap with thecenter of the iron-induced absorption band formed around 1100 nm.

5. A method (100) as in any one of the preceding claims, characterized in step(102) adjusting the power of the light transmitted from the light source characterized in that the power of the light transmitted from the light source is controlled by means of a neutral density filter or any power regulating component, and characterized in that the power control enables the laser pulse energy to be varied for constant pulse width and repetition rate.

6. A method (100) as in any one of the preceding claims, characterized in step(103) of adjusting the beam diameter and transmitting it to the focusing lens, characterized in that a telescope system or a beam expander is used for adjusting the beam diameter and transmitting the beam from there to the focusing lens.

7. A method (100) as in claim 6, characterized in that the NA of the focusing lens, used in the step (104) of obtaining modifications embedded in the glass by positioning the beam from the focusing lens in the glass and adjusting the scanning direction and speed, is at least 0.30.

8. A method (100) as in claim 6 or 7, characterized in the step (104) of obtaining the modifications embedded in the glass by positioning the beam from the focusing lens in the glass and adjusting the scanning direction and speed, wherein the silicate glasses are inscribed in their bulk by transverse or longitidunal laser scanning.

9. A method (100) as in any one of claims 5-8, characterized in step (104) of obtaining modifications embedded in the glass by positioning the beam from the focusing lens in the glass and adjusting the scanning direction and speed, characterized in that the size of the generated structural elements is controlled by the appropriate choice of polarization, scanning speed and direction, and power.

10. A method (100) as in any one of claims 5-9, characterized in that in step (104) of obtaining modifications embedded in the glass by positioning the beam from the focusing lens in the glass and adjusting the scanning direction and speed, a high degree of control over the depth and position of the micro-modifications in glass sample makes it possible to arrange these micro-modifications(s) in various architectures, in the form of single-line, mesh type arrays, multi-layered mesh type arrays or various curved architectures inside the glass.

11. A method (100) as in any one of the claims 5-10, characterized in that in the step of splitting / cutting (105) of laser etched glass to obtain a pristine and uncontaminated interface prior to chemical etching, the splitting / cutting step can be achieved by diamond-based cutting, CO2 laser notch-less cutting, filamentation-based cutting, laser ablation-based cutting, or any variation thereof.

12. A method (100) as in any one of the preceding claims, characterized in step (106) of using a recipe for selective chemical pre-etching of high-aspect- ratio micro-channels in glass, characterized in that, after the samples are cleaved / cut, an HF solution having a molarity concentration of 1.5-5 mol / L is used to pre-etch the samples, and the pre-etching time is between 30 and 120 s.

13. A method (100) as in claim 12, characterized in step (107) of using a recipe for selective chemical etching of high-aspect-ratio micro-channels in glass, wherein an aqueous NaOH solution having a concentration in the range of 7-12 mol / L is used as the main etchant to selectively etch modifications in soda silicate glasses for a period of at least 1 hour and at a temperature of at least 60°C.

Citation Information

Patent Citations

  • Method and device for manufacturing three-dimensional micro-channel in PMMA (polymethyl methacrylate) by using femtosecond laser

    CN103831536A

  • Method for manufacturing micro channel by combining laser polarization selective ablation with acid etching

    CN104625438A

  • Ultrafast laser direct writing method for modifying existing microstructures on a submicron scale

    US20050191771A1