Preparation method of antioxidant sanshool polymer material and its application in skin repair
By introducing marsaicin into the lipoic acid system, antioxidant marsaicin polymer materials are prepared, which solves the problems of lipoic acid instability and functional loss, and achieves rapid healing and long-term stable treatment of diabetic ulcers.
Patent Information
- Application Number
- CN202210800906.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-07-08
AI Technical Summary
Lipoic acid has instability and potential risks as a therapeutic drug for diabetes ulcers, and the loss of functional motifs during polymerization leads to weakening of antioxidant capacity, making it difficult to effectively heal diabetes ulcers in the long term.
The natural pepper extract of yamsaicin with good antioxidant properties is introduced into the lipoic acid system, and the antioxidant yamsaicin polymer material is prepared through esterification reaction and thermal polymerization to construct polylipoic acid-yamsaicin material to ensure the oxidative stress regulation ability and stability.
The prepared antioxidant yamsaicin polymer material has excellent antioxidant stability and biocompatibility, which can quickly repair diabetic ulcers, prolong the action time, reduce potential risks, and significantly improve the healing efficiency of diabetic ulcers.
Smart Images

Figure CN116144024B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of natural molecule macromolecules, and particularly relates to a preparation method of an antioxidant sanshool polymer material and its application in skin repair. Background Art
[0002] Diabetic ulcers are a complication of diabetes, which often occur in the feet of patients, so they are also called diabetic foot. Due to diabetes, patients suffer from neuropathy in their blood vessels. Excessive blood sugar levels in the body interfere with the oxidation reaction of protein glucose to produce oxygen free radicals. These destructive active oxygen free radicals continue to accumulate in the body and cannot be metabolized in time, thereby causing oxidative stress to damage tissues and cells, leading to microvascular and nerve lesions and forming difficult-to-heal ulcers. This will bring great inconvenience and distress to patients, so it is very necessary to study how to accelerate the healing process of diabetic wound ulcers.
[0003] A large number of clinical and research results in the early stage have shown that lipoic acid can effectively treat diabetic neuropathy. Therefore, a large number of studies have been conducted on the use of lipoic acid to treat diabetic foot at home and abroad, and it has been found that lipoic acid has a certain promoting effect on accelerating the healing process of diabetic ulcer wounds. The main conclusion can be attributed to the fact that lipoic acid has the effect of scavenging excessive reactive oxygen free radicals and inhibiting oxidative stress reactions, which can effectively regulate the oxidative environment of the affected area and maintain a relative oxidative balance, thereby preventing and treating peripheral vascular lesions, effectively improving microcirculatory disorders and neuropathy, and thus improving the cure rate of diabetic foot.
[0004] However, lipoic acid is a small molecule compound, and this inherent property determines that it has certain instability, short action cycle, potential risks of use, etc. Based on its fast effect and short duration, lipoic acid needs to be supplemented frequently when used as a therapeutic drug, which will result in a higher cumulative dosage. However, studies have shown that overdose may cause a serious burden on the liver and kidneys, so there are certain potential risks. Polymers have the characteristics of long action time, good biocompatibility, and low potential risks. Therefore, the development of lipoic acid-based polymers for the treatment of diabetic ulcers has certain value. However, during the polymerization process, lipoic acid will lose some of its functional elements, which will weaken its antioxidant capacity to a certain extent. Summary of the invention
[0005] In order to solve the deficiencies mentioned in the background technology, the present invention introduces sanshool, a natural pepper extract with good antioxidant properties, into a lipoic acid polymer system, and provides a preparation method of an antioxidant sanshool polymer material and its application in skin repair.
[0006] The invention introduces sanshool, a natural pepper extract with good antioxidant properties, into a lipoic acid polymer system to construct a polylipoic acid-sanshool material. The method of the invention is efficient and controllable, and the obtained product can ensure good oxidative stress regulation ability and good stability, and has a long action time, good biocompatibility, and the ability to accelerate the healing of diabetic ulcers, and has good application prospects.
[0007] The invention grafts sanshool onto polylipoic acid to prepare an antioxidant sanshool polymer material. Polylipoic acid is first prepared by thermal polymerization, and then sanshool is grafted onto polylipoic acid by esterification reaction to obtain a polylipoic acid-sanshool material; or sanshool and lipoic acid are first grafted by coupling by esterification reaction, and then thermal polymerization is performed to obtain the polylipoic acid-sanshool material.
[0008] The technical solution of the present invention is:
[0009] The preparation method of the antioxidant sanshool polymer material comprises: grafting sanshool to polylipoic acid through an esterification reaction of sanshool and polylipoic acid to obtain the sanshool polymer material; or grafting sanshool to lipoic acid through an esterification reaction of sanshool and lipoic acid, and then polymerizing the grafted lipoic acid to obtain the sanshool polymer material.
[0010] In some specific embodiments, polylipoic acid is obtained by thermal polymerization of lipoic acid, the thermal polymerization temperature is 40 to 90° C., and the thermal polymerization time is 1 to 6 hours.
[0011] In some specific embodiments, the esterification reaction of sanshool and polylipoic acid is specifically as follows:
[0012] Under the catalysis of 4-dimethylaminopyridine and N,N'-diisopropylcarbodiimide, 1 part by mass of polylipoic acid and 0.5-2.0 parts by mass of sanshool are subjected to esterification reaction for 16-36 hours, so that sanshool is grafted onto polylipoic acid; wherein, the amount of 4-dimethylaminopyridine is 0.2-0.6 parts by mass, and the amount of N,N'-diisopropylcarbodiimide is 2.0-4.0 parts by mass.
[0013] In some specific embodiments, the esterification reaction of sanshool and lipoic acid is specifically as follows:
[0014] Under the catalysis of 4-dimethylaminopyridine and N,N'-diisopropylcarbodiimide, 1 part by mass of lipoic acid and 0.5-2.0 parts by mass of sanshool are subjected to esterification reaction for 16-36 hours to graft sanshool onto lipoic acid; wherein, the amount of 4-dimethylaminopyridine is 0.2-0.6 parts by mass, and the amount of N,N'-diisopropylcarbodiimide is 2.0-4.0 parts by mass.
[0015] In some specific embodiments, the grafted lipoic acid is polymerized by thermally polymerizing the grafted lipoic acid at a temperature of 40 to 90° C. for a time of 1 to 6 hours.
[0016] The prepared antioxidant sanshool polymer material has excellent antioxidant stability, can promote the rapid repair of diabetic ulcer wounds, and can be used for preparing diabetic ulcer wound repair agents.
[0017] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0018] (1) The present invention rationally analyzes the molecular structure from a chemical perspective, and prepares polylipoic acid-sanshool materials through two strategies: polymerization first and then grafting, and grafting first and then polymerization, which has excellent application value.
[0019] (2) The polymerization method adopted in the present invention is thermal polymerization, which is easy to operate and has high efficiency.
[0020] (3) The molecular weight and molecular weight distribution can be adjusted by adjusting the thermal polymerization temperature, and it has good adjustable and controllable properties.
[0021] (4) The prepared polylipoic acid-sanshool material has good DPPH free radical scavenging ability and ABTS free radical scavenging ability, and can cope with a variety of oxidative stress microenvironments.
[0022] (5) The prepared polylipoic acid-sanshool material has good biocompatibility, which lays the foundation for its biological application.
[0023] (6) The prepared polylipoic acid-sanshool material has good antioxidant capacity at the cellular level and can successfully transform its physical and chemical properties into biological properties.
[0024] (7) The prepared polylipoic acid-sanshool material has the effect of accelerating the healing process of diabetic ulcers, laying a foundation for its further exploration of biological applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is the molecular weight of polylipoic acid-sanshool obtained at different polymerization temperatures in Example 1;
[0026] Figure 2 The molecular weight distribution of polylipoic acid-sanshool obtained at different polymerization temperatures in Example 1;
[0027] Figure 3 is the molecular weight of polylipoic acid-sanshool obtained at different polymerization temperatures in Example 2;
[0028] Figure 4The molecular weight distribution of polylipoic acid-sanshool obtained at different polymerization temperatures in Example 2;
[0029] Figure 5 DPPH free radical scavenging curves of samples PTAS-1 and PTAS-2;
[0030] Figure 6 The DPPH antioxidant stability of samples sanshool, PTA+S, TA+S, PTAS-1, and PTAS-2;
[0031] Figure 7 ABTS free radical scavenging curves of samples PTAS-1 and PTAS-2;
[0032] Figure 8 The ABTS antioxidant stability of samples sanshool, PTA+S, TA+S, PTAS-1, and PTAS-2;
[0033] Fig. 9 The cell compatibility of samples PTAS-1 and PTAS-2 at different concentrations;
[0034] Fig.10 The results of cell antioxidant experiments of samples PTAS-1 and PTAS-2 at different concentrations;
[0035] Fig.11 The results of samples PTAS-1 and PTAS-2 accelerating the wound healing process of diabetic ulcers. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention will be further described in detail below in combination with specific implementation methods and examples. It should be understood that the embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0037] The preparation method of the antioxidant sanshool polymer material comprises: grafting sanshool to polylipoic acid through an esterification reaction of sanshool and polylipoic acid to obtain the sanshool polymer material; or grafting sanshool to lipoic acid through an esterification reaction of sanshool and lipoic acid, and then polymerizing the grafted lipoic acid to obtain the sanshool polymer material.
[0038] A specific implementation step of the method for preparing the antioxidant sanshool polymer material of the present invention is as follows:
[0039] (110) preparing polylipoic acid by thermal polymerization of lipoic acid, wherein the thermal polymerization temperature is 40-90°C and the thermal polymerization time is 1-6 h;
[0040] (120) Under the catalysis of 4-dimethylaminopyridine and N,N'-diisopropylcarbodiimide, 1 part by mass of polylipoic acid and 0.5-2.0 parts by mass of sanshool are subjected to an esterification reaction for 16-36 hours to graft sanshool onto polylipoic acid; in this specific embodiment, 0.2-0.6 parts by mass of 4-dimethylaminopyridine and 2.0-4.0 parts by mass of N,N'-diisopropylcarbodiimide are commonly used esterification reaction catalysts, which are used to promote the esterification reaction between the carboxyl group of polylipoic acid and the hydroxyl group of sanshool;
[0041] (130) The reactant of step (120) is dialyzed at a molecular weight cut-off (MWCO) of 3200 Da for 2 to 4 days, and then freeze-dried to obtain a polylipoic acid-sanshool material.
[0042] Another specific implementation step of the method for preparing the antioxidant sanshool polymer material of the present invention is as follows:
[0043] (210) Under the catalysis of 4-dimethylaminopyridine and N,N'-diisopropylcarbodiimide, 1 part by mass of thioctic acid and 0.5-2.0 parts by mass of sanshool are subjected to an esterification reaction for 16-36 hours to graft sanshool onto thioctic acid; in this specific embodiment, 0.2-0.6 parts by mass of 4-dimethylaminopyridine and 2.0-4.0 parts by mass of N,N'-diisopropylcarbodiimide are commonly used esterification reaction catalysts, which are used to promote the esterification reaction between the carboxyl group of thioctic acid and the hydroxyl group of sanshool;
[0044] (220) Purifying the product of step (210), including precipitation, centrifugation, and washing.
[0045] (230) The purified product was subjected to thermal polymerization at a temperature of 40–90 °C for 1–6 h to obtain polylipoic acid-sanshool material.
[0046] The polylipoic acid-sanshool material prepared by the present invention has good and stable DPPH and ABTS free radical scavenging ability, good biocompatibility and cell antioxidant ability, and can accelerate the healing of diabetic ulcer wounds.
[0047] Several embodiments and comparative examples are provided below. In the embodiments and comparative examples, lipoic acid was purchased from Shanghai Anaiji Chemical Co., Ltd. with a purity of 98.0%; 4-dimethylaminopyridine was purchased from Shanghai Anaiji Chemical Co., Ltd. with a purity of 98%; N,N'-diisopropylcarbodiimide was purchased from Shanghai Anaiji Chemical Co., Ltd. with a purity of 98%; sanshool was hydroxy-α-sanshool, purchased from Nanjing Dausif Biotechnology Co., Ltd. with a purity of 95%, CAS No.: 83883-10-7.
[0048] Example 1
[0049] This embodiment adopts the strategy of first polymerization and then grafting to prepare polylipoic acid-sanshool material, and the specific steps are as follows:
[0050] (1) thioctic acid is placed in a round-bottom flask and heated by an oil bath method at 40°C, 50°C, 60°C, 70°C, 80°C, and 90°C, respectively, for 4 hours. It can be observed that after heating, the thioctic acid solid powder is transformed into a light yellow viscous liquid, indicating that a certain degree of polymerization reaction has been carried out. This step obtains 6 groups of polylipoic acid polymerized at different polymerization temperatures, and 1 mass part of each group of polylipoic acid is taken to prepare a polylipoic acid-sanshool material according to steps (2) to (3);
[0051] (2) Dissolve 1 part of polylipoic acid in N,N-dimethylformamide (DMF) to prepare a polylipoic acid solution with a concentration of 30 mg / mL, add 1.2 parts of sanshool, 0.4 parts of 4-dimethylaminopyridine (DMAP), and 3.5 parts of N,N'-diisopropylcarbodiimide (DIPC), and stir at room temperature for 24 h in a closed environment;
[0052] (3) After the reaction is completed, the solvent DMF is removed by vacuum distillation, and the obtained product is dialyzed, with a molecular weight cut-off MWCO=3200Da, ethanol as the dialysate, and the dialysis time is 3 days. The solution after the dialysis is then freeze-dried to obtain a polylipoic acid-sanshool material.
[0053] The molecular weight and molecular weight distribution of polylipoic acid-sanshool materials obtained at different polymerization temperatures were characterized by gel permeation chromatography. Figure 1 ,from Figure 1 It can be seen that as the polymerization temperature increases, the molecular weight of the polymer gradually increases. The molecular weight increases rapidly below 70°C, and increases slowly above 70°C. Figure 2 ,from Figure 2It can be seen that the molecular weight distribution is narrow below 70°C, and the molecular weight distribution becomes rapidly broad above 70°C, which may be caused by the micro-crosslinking phenomenon generated at high temperature. Combining the characteristics of molecular weight and molecular weight distribution, the polylipoic acid-sanshool material obtained at a polymerization temperature of 70°C was selected for subsequent characterization and named sample PTAS-1.
[0054] Example 2
[0055] This embodiment adopts the strategy of grafting first and then polymerization to prepare polylipoic acid-sanshool material, and the specific steps are as follows:
[0056] (1) Dissolve 1 part by mass of lipoic acid in N,N-dimethylformamide to prepare a 30 mg / mL lipoic acid solution, add 1.2 parts by mass of sanshool, 0.4 parts by mass of 4-dimethylaminopyridine (DMAP), and 3.5 parts by mass of N,N'-diisopropylcarbodiimide (DIPC), and stir at room temperature for 24 hours in a closed environment;
[0057] (2) precipitating the product obtained in step (1) with deionized water, centrifuging, and washing three times to remove unreacted substances and a small amount of by-products; then freeze-drying the precipitate to obtain a yellow powder, i.e., the coupling product of sanshool and lipoic acid;
[0058] (3) The coupling product was placed in a glass round-bottom flask and heated using an oil bath method. The heating temperatures were 40°C, 50°C, 60°C, 70°C, 80°C, and 90°C, respectively, and the heating time was 4 h. It can be observed that after heating, the coupling product powder turned into a yellow viscous liquid, indicating that a certain degree of polymerization reaction occurred at the six polymerization temperatures.
[0059] The molecular weight and molecular weight distribution of polylipoic acid-sanshool materials obtained at 6 different polymerization temperatures were characterized by gel permeation chromatography. Figure 3 ,from Figure 3 It can be seen that as the polymerization temperature rises, the molecular weight of the polymer gradually increases. The molecular weight increases rapidly below 70°C, and increases slowly above 70°C. Figure 4 ,from Figure 4 It can be seen that the molecular weight distribution is narrow below 70°C, and the molecular weight distribution becomes rapidly broadened above 70°C. This has a similar trend to the polylipoic acid-sanshool material obtained by the strategy of first polymerization and then grafting, which is determined by the intrinsic characteristics of the lipoic acid polymerization process. The polylipoic acid-sanshool material obtained by the polymerization temperature of 70°C is preferred for subsequent characterization and is named sample PTAS-2.
[0060] Example 3
[0061] In this example, the 2,2-diphenyl-1-picrylhydrazyl (DPPH) method was used to evaluate the in vitro DPPH free radical scavenging ability and antioxidant stability of samples PTAS-1 and PTAS-2.
[0062] (1) In vitro DPPH free radical scavenging ability of samples.
[0063] Prepare sample solution: prepare 0.1mmol / L DPPH ethanol solution, and prepare 1mg / mL PTAS-1 and PTAS-2 material solutions. Take 300μL of DPPH solution and dilute it with an appropriate amount of ethanol, then add 60μL of sample solution to keep the final volume of the solution at 3mL, and obtain a sample solution with a concentration of 20μg / mL. The absorbance at 517nm is used to evaluate the free radical scavenging effect. The absorbance is measured at different time points within 30 minutes to obtain the free radical scavenging curve. The results are shown in Figure 5 .from Figure 5 It can be seen that the sample PTAS-2 obtained by the strategy of grafting first and then polymerization has better free radical scavenging ability. This is because the different preparation strategies bring a higher loading amount of sanshool, which ultimately makes it have stronger antioxidant ability.
[0064] (2) DPPH antioxidant stability of samples.
[0065] The sample preparation method is the same as above, and the absorbance at 517nm is used to evaluate the free radical scavenging rate. The free radical scavenging rate of the sample is measured after being kept in the dark and stirred for 30 minutes at room temperature. Afterwards, the sample is irradiated for 4 hours under simulated sunlight with a power of 1.5W, and the absorbance of each sample at 517nm is measured again to evaluate the free radical scavenging rate after irradiation, and the antioxidant stability is calculated: Antioxidant stability (%) = free radical scavenging rate after irradiation / free radical scavenging rate before irradiation × 100%.
[0066] Sanshool, a mixture of sanshool and polylipoic acid (named as sample PTA+S), and a mixture of sanshool and lipoic acid (named as sample TA+S) were used as control samples. Sample PTA+S was obtained by mixing 1.2 parts by mass of sanshool and 1 part by mass of polylipoic acid, and sample TA+S was obtained by mixing 1.2 parts by mass of sanshool and 1 part by mass of lipoic acid. The antioxidant stability of each control sample was determined by the aforementioned method. The antioxidant stability of each sample and each control sample is shown in Figure 6 ,from Figure 6 It can be seen that the antioxidant stability of sanshool is poor, and the antioxidant stability of samples PTAS-1 and PTAS-2 prepared by the method of the present invention are effectively improved, among which the antioxidant stability of sample PTAS-1 is better; but the antioxidant stability of the mixture of sanshool and polylipoic acid and the mixture of sanshool and lipoic acid cannot be effectively improved.
[0067] Example 4
[0068] In this example, the 2,2'-azinobis(3-ethylbenzothiazoline-6-sulfonic acid) diammonium salt (ABTS) method was used to evaluate the aqueous phase free radical scavenging ability and antioxidant stability of samples PTAS-1 and PTAS-2.
[0069] (1) Aqueous phase free radical scavenging ability of samples.
[0070] An ABTS aqueous solution with a concentration of 7 mmol / L and an aqueous potassium persulfate solution with a concentration of 2.45 mmol / L were prepared respectively; the ABTS aqueous solution and the potassium persulfate aqueous solution were mixed at a molar ratio of 1:2, and allowed to stand overnight at room temperature so that they were in a dark state to obtain an ABTS detection reagent.
[0071] Prepare sample solution: Prepare PTAS-1 and PTAS-2 sample solutions with a concentration of 1 mg / mL. Take 100 μL of ABTS detection reagent solution and dilute it with an appropriate amount of deionized water, then add 60 μL of sample solution to keep the final volume of the solution at 3 mL to obtain a sample solution with a concentration of 20 μg / mL. The absorbance at 734 nm was used to evaluate the free radical scavenging effect. The absorbance was measured at different time points within 30 minutes to obtain the free radical scavenging curve, see Figure 7 .from Figure 7 It can be seen that samples PTAS-1 and PTAS-2 both have scavenging rates consistent with the DPPH free radical scavenging ability, among which sample PTAS-2 has better free radical scavenging ability.
[0072] (2) ABTS antioxidant stability of samples.
[0073] The sample preparation method is the same as above, and the absorbance at 734nm is used to evaluate the free radical scavenging rate. The free radical scavenging rate of the sample is measured after being kept in the dark and stirred for 30 minutes at room temperature. Afterwards, the sample is irradiated for 4 hours under simulated sunlight with a power of 1.5W, and the absorbance of each sample at 734nm is measured again to evaluate the free radical scavenging rate after irradiation, and the antioxidant stability is calculated: Antioxidant stability (%) = free radical scavenging rate after irradiation / free radical scavenging rate before irradiation × 100%.
[0074] Sanshool, a mixture of sanshool and polylipoic acid (named as sample PTA+S), and a mixture of sanshool and lipoic acid (named as sample TA+S) were used as control samples. Sample PTA+S was obtained by mixing 1.2 parts by mass of sanshool and 1 part by mass of polylipoic acid, and sample TA+S was obtained by mixing 1.2 parts by mass of sanshool and 1 part by mass of lipoic acid. The antioxidant stability of each control sample was determined by the aforementioned ABTS method. The antioxidant stability of each sample and each control sample is shown in Figure 8,from Figure 8 It can be seen that the antioxidant stability of sanshool is poor, and the antioxidant stability of samples PTAS-1 and PTAS-2 prepared by the method of the present invention are effectively improved, among which sample PTAS-1 has better stability; the antioxidant stability of the mixture of sanshool and polylipoic acid and the mixture of sanshool and lipoic acid cannot be effectively improved.
[0075] Example 5
[0076] The biocompatibility of samples PTAS-1 and PTAS-2 was tested.
[0077] NIH mouse embryonic fibroblast 3T3 cells were used as cell lines, and the MTT colorimetric method was used to verify the cytotoxicity of the samples. The cells were cultured by adding 10% fetal bovine serum (FBS) to DMEM culture medium for co-incubation. The culture atmosphere was a humid atmosphere containing 5% CO2, and the temperature was maintained at 37°C. The cultured NIH 3T3 cells were incubated in a 96-well plate at a density of 2000 cells per well for 24 hours, and then treated with 50 and 100 μg / mL samples for another 24 hours. Then, the corresponding cell survival rate was detected according to the MTT colorimetric test instructions. The test results are shown in Fig. 9 .from Fig. 9 It can be seen that at the concentrations of 50 and 100 μg / mL, samples PTAS-1 and PTAS-2 have good biocompatibility and good biological application prospects.
[0078] Example 6
[0079] The NIH 3T3 cells cultured in Example 5 were inoculated into a 12-well plate at 100,000 / well and incubated in the well plate for 24 hours. After the incubation was completed, the culture medium was removed, and 500 μL of DMEM culture medium containing different concentrations of PTAS-1 and PTAS-2 materials was added, and 500 μL of full-component culture medium and 100 μL of diluted hydrogen peroxide (concentration of 100 μmol / L) were further added. Then the culture medium was removed, 200 μL of trypsin was added to digest the cells and 200 μL of culture medium was added to terminate the trypsin digestion; the supernatant was removed by centrifugation, 1 ml of PBS solution was added to resuspend, and then 250 μL of the prepared probe was added; the cell sample was finally resuspended in PBS after centrifugation, and quantitative analysis was performed using a flow cytometer. The analysis time was 24 hours, and the obtained results were Fig.10 As shown in Figure 10, compared with the positive control, the intensity of the materials with different concentrations decreased, and the higher the concentration, the greater the decrease; in addition, the fluorescence intensity of sample PTAS-2 was lower than that of sample PTAS-1, showing its better antioxidant capacity, which is consistent with the antioxidant capacity results of the above DPPH and ABTS tests.
[0080] Example 7
[0081] This example measures the ability of samples PTAS-1 and PTAS-2 to accelerate wound healing of diabetic ulcers.
[0082] Rats were fed a high-sugar and high-fat diet and a low-dose of streptozotocin to establish a full-thickness skin defect model on the foot of type II diabetic SD rats. After the model was successfully established, all rats were randomly divided into 3 groups, including a control group, a PTAS-1 group, and a PTAS-2 group, with 5 rats in each group. After standard anesthesia procedures, a puncture biopsy needle was used to form a circular skin wound with a diameter of 5 mm on the dorsal foot of the rat. After removing the wound skin, 50 μL of PBS buffer was added to the wound of the control group. Each 50 μL PTAS-1 and PTAS-2 sample was added to the wound of the experimental group. On the 14th day, rats in each group were anesthetized according to standard procedures, the wound was photographed, and the images were processed by Image J software to measure the wound area. The data are shown in Figure 1. Fig.11 .from Fig.11 It can be seen that the application of the material can effectively promote the wound healing process, among which the sample PTAS-2 with stronger antioxidant capacity accelerates the healing process the fastest, which provides a solid foundation for its application in the treatment of diabetic ulcers.
[0083] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the invention disclosed herein. This application is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not disclosed by the present invention. The specification and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the following claims.
[0084] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. The preparation method of the antioxidant sanshool polymer material is characterized in that: By esterification reaction of sanshool and polylipoic acid, sanshool is grafted onto polylipoic acid to obtain sanshool polymer material; or by esterification reaction of sanshool and lipoic acid, sanshool is grafted onto lipoic acid, and then the grafted lipoic acid is polymerized to obtain sanshool polymer material; The specific esterification reaction of sanshool and polylipoic acid is as follows: Under the catalysis of 4-dimethylaminopyridine and N,N'-diisopropylcarbodiimide, 1 part by mass of polylipoic acid and 0.5-2.0 parts by mass of sanshool are subjected to esterification reaction for 16-36 hours, so that sanshool is grafted onto polylipoic acid; wherein the amount of 4-dimethylaminopyridine is 0.2-0.6 parts by mass, and the amount of N,N'-diisopropylcarbodiimide is 2.0-4.0 parts by mass; The specific esterification reaction of sanshool and lipoic acid is: Under the catalysis of 4-dimethylaminopyridine and N,N'-diisopropylcarbodiimide, 1 part by mass of lipoic acid and 0.5-2.0 parts by mass of sanshool are subjected to esterification reaction for 16-36 hours, so that sanshool is grafted onto lipoic acid; wherein the amount of 4-dimethylaminopyridine is 0.2-0.6 parts by mass, and the amount of N,N'-diisopropylcarbodiimide is 2.0-4.0 parts by mass; The step of polymerizing the grafted lipoic acid specifically comprises: subjecting the grafted lipoic acid to thermal polymerization at a temperature of 40 to 90° C. for a time of 1 to 6 hours.
2. the preparation method of antioxidant sanshool polymer material as claimed in claim 1, is characterized in that: The polylipoic acid is obtained by thermal polymerization of lipoic acid, the thermal polymerization temperature is 40-90° C., and the thermal polymerization time is 1-6 hours.