A M-WOxZnOZrO2 catalyst and its application in preparing diisobutylene
The preparation of diisobutene in isobutene reaction through M-WOxZnOZrO2 solid solution super acid catalyst solves the problems of low selectivity and complex separation process in the prior art, and achieves a catalytic effect with high selectivity and activity, and is environmentally friendly and cost-effective in the process. Low.
Patent Information
- Application Number
- CN202211617919.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-15
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-12-15
AI Technical Summary
In the prior art, the selectivity of diisobutene and the complex separation process lead to low catalytic activity and diisobutene selectivity, making it difficult to achieve efficient preparation.
The M-WOxZnOZrO2 solid solution super acid catalyst was prepared by impregnation, precipitation or sol-gel method. The ZnOZrO2 solid solution was used as a carrier and WOx was used as a super acid component, combined with the template agent and the precipitant agent to prepare high activity and selectivity. Catalyst and catalyze isobutene to form diisobutene in the reactor.
It achieves a catalytic effect with high selectivity and activity, mild reaction conditions, no equipment corrosion, simple and environmentally friendly process, reduces production costs, and avoids waste acid and wastewater treatment.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of petrochemical industry, and particularly relates to an M-WOxZnOZrO2 catalyst and application thereof in preparing diisobutylene. Technical Background
[0002] The main components of diisobutylene (diisobutylene) are 2,4,4-trimethyl-1-pentene and 2,4,4-trimethyl-2-pentene. Diisobutylene is mainly used to produce octylphenol and isooctyl alcohol. As an important organic chemical raw material, it can undergo self-polymerization or copolymerization, addition reaction, halogenation reaction, alkylation reaction, carbonylation reaction, etc., because of its C=C double bond, to generate a series of fine chemical intermediates, which are widely used in plastic additives, rubber additives, lubricants, antioxidants, surfactants, synthetic detergents and other fields.
[0003] In industry, diisobutylene is usually used for dimerization of C4 olefins to produce high-octane gasoline. There are few studies on the process of selective dimerization of isobutylene with diisobutylene as the target product. Usually, isobutylene in mixed C4 is dimerized under the action of an acid catalyst to produce diisobutylene. At present, a variety of diisobutylene production methods have been developed, mainly including sulfuric acid extraction method, solid phosphoric acid method, molecular sieve method or resin method, etc. Among them, the industrialized production technologies include sulfuric acid extraction process, Bayer butene dimerization process, Diermersol X dimerization process, Octol butene dimerization process, Catstil catalytic distillation process, etc. Most of them are aimed at removing isobutylene in mixed C4 or producing mixed C8 olefins (diisobutylene, dimer of normal butene and normal and isobutylene co-dimers, etc.) or isobutylene oligomers. It is difficult to obtain high-purity diisobutylene in the above processes, and the process is complicated. The equipment of some processes is seriously corroded.
[0004] Since the use of liquid acid catalysts is subject to many restrictions, people have focused on the research of new solid acid catalysts. To date, solid acid catalysts used for isobutylene polymerization reactions mainly include macroporous sulfonic acid resin catalysts, solid phosphoric acid catalysts, molecular sieve catalysts, solid superacid catalysts, oxides and oxide complex catalysts. The solid phosphoric acid method is a commonly used method in industry. The raw material is isobutylene in mixed C4. Solid phosphoric acid is used as a catalyst to carry out dimerization in a fixed bed reactor. The selectivity can reach 75% (Yao Yaping, Yuan Meiqing, Xu Jing, etc., "T-49 New Solid Phosphoric Acid Catalyst and Application" "Petroleum Refining and Chemical Industry", 2000, 31 (1) P10). Patent CN1810742A discloses a method for preparing diisobutylene using free phosphoric acid as a catalyst, and the diisobutylene selectivity can reach more than 80%. Patent EP0371938A discloses a solid phosphoric acid catalyst with silicon dioxide as a carrier, but the patent does not describe the raw materials and give a specific dimer selectivity. Patent WO01046095A1 discloses a Hβ molecular sieve as a catalyst for the production of diisobutylene by the superposition of mixed C4 olefins. It is found that the silicon-aluminum ratio has a great influence on the product distribution. When the Hβ silicon-aluminum ratio is 100, the isobutylene conversion rate is 100%, the diisobutylene selectivity is 48%, and the deactivation is very fast. Patent CN1087616A discloses an aluminum silicate catalyst for the dimerization reaction of C4 fraction isobutylene, and the dimer selectivity is 65%. Gonzalez et al. (Catalysis Letters. 2006, 110: 107-113) studied Ni 2+ The effect of modified zeolite molecular sieves on isobutylene dimerization. The authors found that the acid content of the molecular sieve can be increased after modification, but the several molecular sieves investigated all have problems such as rapid deactivation and low conversion rate. Patent CN104395265A discloses a method for preparing isobutylene by fermentation of sugar and dimerization to produce diisobutylene, but no specific selectivity results are given. Patent CN104815695B discloses a method for preparing diisobutylene using carbon nanotube-supported ionic liquid catalysts, but the preparation of this method is too complicated and not conducive to industrial application. Patent CN206622082U discloses a device for preparing diisobutylene, triisobutylene and tetraisobutylene by polymerization of isobutylene. The device structure in this method is simple and the stirring is uniform.
[0005] As can be seen from the above, solid acid catalysts have been used in the preparation of diisobutylene by isobutylene polymerization, but there are problems such as low catalytic activity and selectivity for diisobutylene. Since the isobutylene polymerization product is widely distributed, the selectivity of diisobutylene is generally improved by reducing the reaction rate of the reaction process, for example, 1) controlling the isobutylene single-pass conversion rate and controlling the polymerization rate to improve the selectivity; 2) reducing the catalyst activity; the above methods all improve the selectivity of diisobutylene by reducing the isobutylene conversion rate. Summary of the invention
[0006] In view of the technical problems of low selectivity and complex separation process of diisobutylene in the prior art, the object of the present invention is to provide an M-WOxZnOZrO2 catalyst and its application in the preparation of diisobutylene. The present invention uses a W-based solid solution superacid as a catalyst and isobutylene as a raw material to prepare diisobutylene. The M-WOxZnOZrO2 prepared by the present invention shows high activity and selectivity.
[0007] To achieve the purpose of the present invention, the following technical solution is provided:
[0008] The invention provides an M-WOxZnOZrO2 solid solution superacid catalyst, wherein M is one or more of La, Ce, Pr, Nd, Pm, Sm, Nb, Sn, Ga, Re, In, Al, Ni, Mn, Mo, Ti and V.
[0009] Based on the above technical solution, further, based on the mass of ZnOZrO2 solid solution, the WOx content is 0.1-30%, the M content is 0.1-20%, and the molar ratio of ZnO to ZrO2 is 10:1-1:20.
[0010] Based on the above technical solution, further, based on the mass of ZnOZrO2 solid solution, the WOx content is 1-20%, and the M content is 1-10%.
[0011] Based on the above technical solution, further, the M-WOxZnOZrO2 solid solution superacid catalyst is prepared by impregnation method, precipitation method and sol-gel method.
[0012] Another aspect of the present invention provides a method for preparing the above-mentioned M-WOxZnOZrO2 solid solution superacid catalyst, which mainly comprises the following steps:
[0013] 1) Weigh a soluble salt of Zn, a soluble salt of Zr and a soluble salt of M, add deionized water and stir to dissolve, to obtain a solution A;
[0014] 2) Weigh W soluble salt, add deionized water and stir to dissolve, to obtain solution B;
[0015] 3) Slowly add solution B to solution A under stirring to obtain solution C after the addition is complete;
[0016] 4) Weigh a certain amount of template, add deionized water, stir for 2-6 hours, slowly add the resulting solution dropwise to solution C, and continue stirring for 2-6 hours after the addition is complete;
[0017] 5) slowly adding a precipitant to the solution obtained in step 4) under stirring at 40-90° C. until the pH is 7-12, and continuing stirring for 1-8 hours;
[0018] 6) transferring the solution obtained in 5) to a hydrothermal reactor and crystallizing at 60-180° C. for 6-48 hours;
[0019] 7) After crystallization, centrifuge and wash, then wash with anhydrous ethanol for 1-5 times, and vacuum dry to obtain a superacid precursor;
[0020] 8) The superacid precursor is calcined at 300-1000° C. in an air atmosphere for 2-12 hours to obtain a M-WOxZnOZrO2 solid solution superacid catalyst.
[0021] Based on the above technical solution, further, the template agent in step 4) is one or more of CTAB, n-butanol, propylene glycol, P123, tetrapropylammonium hydroxide, Tween, and PEG2000, and the ratio of the total molar number of the template agent to the metal ion is 1:1-1:20.
[0022] Based on the above technical solution, further, the precipitant in step 5) is one or more of NH4HCO3, (NH4)2CO3, Na2CO3, NaOH, ammonia water or urea, and the dropping speed is 1-5 ml / min.
[0023] Based on the above technical solution, further, in step 6), the crystallization temperature is 70-100° C., and the crystallization time is 6-24 h.
[0024] Based on the above technical solution, further, in step 7), the vacuum drying temperature is 50-80°C, and the vacuum drying time is 24-48h.
[0025] Based on the above technical solution, further, in step 8), the calcination temperature is 400-600° C., and the calcination time is 4-10 h.
[0026] The present invention also provides a method for preparing diisobutylene by polymerizing isobutylene, which utilizes the above-mentioned M-WOxZnOZrO2 solid solution superacid catalyst to catalyze the reaction of isobutylene in a reactor / fixed bed to prepare diisobutylene.
[0027] Based on the above technical solution, further, the reaction temperature is 40-100° C., the reaction pressure is 0.1-5.0 MPa, the reaction time is 2-10 h, and the mass ratio of the catalyst to isobutylene is 1:10-1:100.
[0028] Based on the above technical solution, further, one or more polar substances selected from methanol, tert-butanol and MTBE are added to the reaction as inhibitors, and the mass ratio of the inhibitor to isobutylene is 1:20-1:200.
[0029] Based on the above technical solution, further, the reaction pressure is the system's own pressure, or the pressure generated by filling with inert gas.
[0030] Compared with the prior art, the present invention has the following advantages:
[0031] 1) The catalyst of the present invention is simple to prepare and has good repeatability, and the reaction selectivity is very high;
[0032] 2) The reaction conditions of the present invention are mild and there is no equipment corrosion;
[0033] 3) The process of the present invention is simple and environmentally friendly, does not generate waste acid and waste water, and does not require waste acid and waste water treatment. It is a true atom-economic reaction and reduces production costs. DETAILED DESCRIPTION
[0034] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0035] Example 1
[0036] Catalyst preparation:
[0037] Weigh 4.46g Zn(NO3)2·6H2O and 18.24g Zr(NO3)4·5H2O, add 100ml deionized water, stir and dissolve to obtain solution A; weigh 1.32g ammonium metatungstate, add 50ml deionized water, stir and dissolve to obtain solution B; slowly drop solution B into solution A under stirring, and obtain solution C after the dropwise addition; weigh 7.29g template CTAB and 8.40g Tween 40 were added with 100mL deionized water and dissolved and stirred for 4h. The obtained solution was slowly added dropwise to solution C. After the addition was completed, stirring was continued for 2h. Under stirring at 70℃, a precipitant of 0.5mol / l (NH4)2CO3 and an equal volume of ammonia water was slowly added dropwise at 3ml / min until the pH was 8.0, and stirring was continued for 2h. The solution was transferred to a hydrothermal autoclave with an inner liner and crystallized for 12h at 80℃. After crystallization, the solution was centrifuged and washed several times, and then washed with anhydrous ethanol for 3 times. The solution was vacuum dried at 80℃ for 48h to obtain a solid solution superacid precursor. The superacid precursor was calcined at 500℃ in an air atmosphere for 6h to obtain a solid solution superacid catalyst WOx / ZnOZrO2.
[0038] Reaction evaluation:
[0039] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0040] Example 2
[0041] Catalyst preparation:
[0042] Weigh 1.45g Ga(NO3)3·9H2O, 4.46g Zn(NO3)2·6H2O, and 18.24g Zr(NO3)4·5H2O, add 100ml deionized water, stir and dissolve to obtain solution A; weigh 1.32g ammonium metatungstate, add 50ml deionized water, stir and dissolve to obtain solution B; slowly drop solution B into solution A under stirring, and obtain solution C after the addition is complete; weigh 8.43g CTAB and 9.36g Tween 40, a template, add 100mL deionized water, dissolve and stir for 4h, and slowly drop the obtained solution into solution C, and continue stirring for 2h after the addition is complete; stir at 70℃ at 3ml / m in slowly dropwise add a precipitant of 0.5 mol / l (NH4)2CO3 and an equal volume of ammonia water until the pH is 8.0, and continue stirring for 2 hours; the solution is transferred to a hydrothermal kettle with an inner liner and crystallized for 12 hours in an environment of 80°C; after crystallization, centrifuge and wash several times, and then wash 3 times with anhydrous ethanol; vacuum dry at 80°C for 48 hours to obtain a solid solution superacid precursor; the superacid precursor is calcined at 500°C in an air atmosphere for 6 hours to obtain a solid solution superacid catalyst Ga-WOx / ZnOZrO2.
[0043] Reaction evaluation:
[0044] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0045] Example 3
[0046] Catalyst preparation:
[0047] Weigh 1.15g La(NO3)3·6H2O, 4.46g Zn(NO3)2·6H2O, and 18.24g Zr(NO3)4·5H2O, add 100ml deionized water, stir and dissolve to obtain solution A; weigh 1.32g ammonium metatungstate, add 50ml deionized water, stir and dissolve to obtain solution B; slowly drop solution B into solution A under stirring, and obtain solution C after the addition is complete; weigh 7.29g CTAB and 8.40g Tween 40, a template, add 100mL deionized water, dissolve and stir for 4h, and slowly drop the solution into solution C, and continue stirring for 2h after the addition is complete; stir at 70℃ at 3ml / m in slowly dropwise add a precipitant of 0.5 mol / l (NH4)2CO3 and an equal volume of ammonia water until the pH is 8.0, and continue stirring for 2 hours; transfer the solution to a hydrothermal kettle with an inner liner, and crystallize for 12 hours in an environment of 80°C; after crystallization, centrifuge and wash several times, and then wash 3 times with anhydrous ethanol; vacuum dry at 80°C for 48 hours to obtain a solid solution superacid precursor; calcine the superacid precursor at 500°C in an air atmosphere for 6 hours to obtain a solid solution superacid catalyst La-WOx / ZnOZrO2.
[0048] Reaction evaluation:
[0049] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0050] Example 4
[0051] Catalyst preparation:
[0052] Weigh 0.81g SnCl4, 4.46g Zn(NO3)2·6H2O, 18.24g Zr(NO3)4·5H2O, add 100ml deionized water and stir to dissolve, to obtain solution A; weigh 1.32g ammonium metatungstate, add 50ml deionized water and stir to dissolve, to obtain solution B; slowly add solution B to solution A under stirring, to obtain solution C after the addition is complete; weigh 7.78g template CTAB and 8.96g Tween 40 were added with 100mL deionized water and dissolved and stirred for 4h. The obtained solution was slowly added dropwise to solution C. After the addition was completed, stirring was continued for 2h. Under stirring at 70℃, a precipitant of 0.5mol / l (NH4)2CO3 and an equal volume of ammonia water was slowly added dropwise at 3ml / min until the pH was 8.0, and stirring was continued for 2h. The solution was transferred to a hydrothermal autoclave with an inner liner and crystallized for 12h at 80℃. After crystallization, the solution was centrifuged and washed several times, and then washed with anhydrous ethanol for 3 times. The solution was vacuum dried at 80℃ for 48h to obtain a solid solution superacid precursor. The superacid precursor was calcined at 500℃ in an air atmosphere for 6h to obtain a solid solution superacid catalyst Sn-WOx / ZnOZrO2.
[0053] Reaction evaluation:
[0054] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0055] Example 5
[0056] Catalyst preparation:
[0057] Weigh 2.13 g C 10 H5B 204.46g Zn(NO3)2·6H2O, 18.24g Zr(NO3)4·5H2O were added to 100ml deionized water and stirred to dissolve to obtain solution A; 1.32g ammonium metatungstate was weighed and added to 50ml deionized water and stirred to dissolve to obtain solution B; solution B was slowly added dropwise to solution A under stirring to obtain solution C after the addition was completed; 8.12g template agent was weighed CTAB and 9.08g Tween 40 were added with 100mL deionized water and dissolved and stirred for 4h. The obtained solution was slowly added dropwise to solution C. After the addition was completed, stirring was continued for 2h. Under stirring at 70℃, a precipitant of 0.5mol / l (NH4)2CO3 and an equal volume of ammonia water was slowly added dropwise at 3ml / min until the pH was 8.0, and stirring was continued for 2h. The solution was transferred to a hydrothermal autoclave with an inner liner and crystallized for 12h at 80℃. After crystallization, the solution was centrifuged and washed several times, and then washed with anhydrous ethanol for 3 times. The solution was vacuum dried at 80℃ for 48h to obtain a solid solution superacid precursor. The superacid precursor was calcined at 500℃ in an air atmosphere for 6h to obtain a solid solution superacid catalyst Nb-WOx / ZnOZrO2.
[0058] Reaction evaluation:
[0059] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0060] Example 6
[0061] Catalyst preparation:
[0062] Weigh 1.12g Nd(NO3)3·6H2O, 4.46g Zn(NO3)2·6H2O, 18.24g Zr(NO3)4·5H2O, add 100ml deionized water, stir and dissolve to obtain solution A; weigh 1.32g ammonium metatungstate, add 50ml deionized water, stir and dissolve to obtain solution B; slowly drop solution B into solution A under stirring, and obtain solution C after the addition is complete; weigh 7.83g CTAB and 8.72g Tween 40, a template, add 100mL deionized water, dissolve and stir for 4h, and slowly drop the obtained solution into solution C, and continue stirring for 2h after the addition is complete; stir at 70℃ at 3ml / m in slowly dropwise add a precipitant of 0.5 mol / l (NH4)2CO3 and an equal volume of ammonia water until the pH is 8.0, and continue stirring for 2 hours; transfer the solution to a hydrothermal kettle with an inner liner, and crystallize for 12 hours in an environment of 80°C; after crystallization, centrifuge and wash several times, and then wash 3 times with anhydrous ethanol; vacuum dry at 80°C for 48 hours to obtain a solid solution superacid precursor; calcine the superacid precursor at 500°C in an air atmosphere for 6 hours to obtain a solid solution superacid catalyst Nd-WOx / ZnOZrO2.
[0063] Reaction evaluation:
[0064] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0065] Example 7
[0066] Catalyst preparation:
[0067] Weigh 5.15g Al(NO3)3·9H2O, 4.46g Zn(NO3)2·6H2O, and 18.24g Zr(NO3)4·5H2O, add 100ml deionized water, stir and dissolve to obtain solution A; weigh 1.32g ammonium metatungstate, add 50ml deionized water, stir and dissolve to obtain solution B; slowly drop solution B into solution A under stirring, and obtain solution C after the addition is complete; weigh 10.21g CTAB and 11.76g Tween 40, a template, add 100mL deionized water, dissolve and stir for 4h, and slowly drop the obtained solution into solution C, and continue stirring for 2h after the addition is complete; stir at 70℃ with 3ml / min, slowly drop a precipitant of 0.5 mol / l (NH4)2CO3 and an equal volume of ammonia water until the pH is 8.0, and continue stirring for 2 hours; transfer the solution to a lined hydrothermal autoclave and crystallize it at 80°C for 12 hours; after crystallization, centrifuge and wash it several times, and then wash it 3 times with anhydrous ethanol; vacuum dry it at 80°C for 48 hours to obtain a solid solution superacid precursor; calcine the superacid precursor at 500°C in an air atmosphere for 6 hours to obtain a solid solution superacid catalyst Al-WOx / ZnOZrO2.
[0068] Reaction evaluation:
[0069] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0070] Example 8
[0071] Catalyst preparation:
[0072] Weigh 1.82g Ni(NO3)2·6H2O, 4.46g Zn(NO3)2·6H2O, 18.24g Zr(NO3)4·5H2O, add 100ml deionized water, stir and dissolve to obtain solution A; weigh 1.32g ammonium metatungstate, add 50ml deionized water, stir and dissolve to obtain solution B; slowly drop solution B into solution A under stirring, and obtain solution C after the addition is complete; weigh 8.75g CTAB and 10.08g Tween 40, a template, add 100mL deionized water, dissolve and stir for 4h, and slowly drop the obtained solution into solution C, and continue stirring for 2h after the addition is complete; stir at 70℃ with 3ml / min, slowly drop a precipitant of equal volumes of 0.5 mol / l (NH4)2CO3 and ammonia water until the pH is 8.0, and continue stirring for 2 hours; transfer the solution to a lined hydrothermal autoclave and crystallize it at 80°C for 12 hours; after crystallization, centrifuge and wash it several times, and then wash it 3 times with anhydrous ethanol; vacuum dry it at 80°C for 48 hours to obtain a solid solution superacid precursor; calcine the superacid precursor at 500°C in an air atmosphere for 6 hours to obtain a solid solution superacid catalyst Ni-WOx / ZnOZrO2.
[0073] Reaction evaluation:
[0074] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0075] Example 9
[0076] Catalyst preparation:
[0077] Weigh 1.15g La(NO3)3·6H2O, 5.15g Al(NO3)3·9H2O, 4.46g Zn(NO3)2·6H2O, 18.24g Zr(NO3)4·5H2O, add 100ml deionized water and stir to dissolve, to obtain solution A; weigh 1.32g ammonium metatungstate, add 50ml deionized water and stir to dissolve, to obtain solution B; slowly add solution B dropwise to solution A under stirring, to obtain solution C after the addition is complete; weigh 10.94g template CTAB and 12.60g Tween 40 were added with 100mL deionized water and dissolved and stirred for 4h. The obtained solution was slowly added dropwise to solution C. After the addition was completed, stirring was continued for 2h. Under stirring at 70℃, a precipitant of 0.5mol / l (NH4)2CO3 and an equal volume of ammonia water was slowly added dropwise at 3ml / min until the pH was 8.0, and stirring was continued for 2h. The solution was transferred to a hydrothermal autoclave with an inner liner and crystallized for 12h at 80℃. After crystallization, the solution was centrifuged and washed several times, and then washed with anhydrous ethanol for 3 times. The solution was vacuum dried at 80℃ for 48h to obtain a solid solution superacid precursor. The superacid precursor was calcined at 500℃ in an air atmosphere for 6h to obtain a solid solution superacid catalyst La-Al-WOx / ZnOZrO2.
[0078] Reaction evaluation:
[0079] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0080] Comparative Example 1
[0081] Catalyst preparation:
[0082] Weigh 4.46g Zn(NO3)2·6H2O and 18.24g Zr(NO3)4·5H2O, add 100ml deionized water and stir to dissolve to obtain solution A; weigh 7.29g template CTAB and 8.40g Tween 40 were added with 100mL deionized water and dissolved and stirred for 4h to obtain solution B. B was slowly added dropwise to solution A and continued to stir for 2h after the addition was completed. Under stirring at 70℃, a precipitant of 0.5mol / l (NH4)2CO3 and an equal volume of ammonia water was slowly added dropwise at 3ml / min until the pH reached 8.0 and continued to stir for 2h. The solution was transferred to a hydrothermal autoclave with an inner liner and crystallized for 12h at 80℃. After crystallization, the solution was centrifuged and washed several times and then washed with anhydrous ethanol for 3 times. The solution was vacuum dried at 80℃ for 48h to obtain a solid solution solid acid precursor. The solid acid precursor was calcined at 500℃ in an air atmosphere for 6h to obtain a solid solution catalyst ZnOZrO2.
[0083] Reaction evaluation:
[0084] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 80°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0085] Comparative Example 2
[0086] Catalyst preparation:
[0087] Weigh 4.46g Zn(NO3)2·6H2O and 18.24g Zr(NO3)4·5H2O, add 100ml deionized water and stir to dissolve to obtain solution A; weigh 7.29g template CTAB and 8.40g Tween 40 were added with 100mL deionized water and dissolved and stirred for 4h to obtain solution B. B was slowly added dropwise to solution A and continued to stir for 2h after the addition was completed. Under stirring at 70℃, a precipitant of 0.5mol / l (NH4)2CO3 and an equal volume of ammonia water was slowly added dropwise at 3ml / min until the pH reached 8.0 and continued to stir for 2h. The solution was transferred to a lined hydrothermal autoclave and crystallized for 12h at 80℃. After crystallization, the solution was centrifuged and washed several times and then washed with anhydrous ethanol for 3 times. The solution was vacuum dried at 80℃ for 48h to obtain a solid solution solid acid precursor. The solid acid precursor was calcined at 500℃ in an air atmosphere for 6h to obtain a solid solution ZnOZrO2. Weigh 1.32g of ammonium metatungstate and add 50ml of deionized water to dissolve it by stirring. Add the above solid solution to the solution and stir overnight. Filter and wash with anhydrous ethanol three times. Dry in an oven at 100℃ for 12h. The solid is calcined at 500℃ in air atmosphere for 4h to obtain a supported solid acid catalyst WOX / ZnOZrO2(ip).
[0088] Reaction evaluation:
[0089] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0090] Comparative Example 3
[0091] Catalyst preparation:
[0092] Weigh 4.46g Zn(NO3)2·6H2O and 18.24g Zr(NO3)4·5H2O, add 100ml deionized water, stir and dissolve to obtain solution A; weigh 1.32g ammonium metatungstate, add 50ml deionized water, stir and dissolve to obtain solution B; slowly drop solution B into solution A under stirring, and obtain solution C after the dropwise addition; weigh 7.29g template CTAB and 8.40g Tween 40 were added with 100mL deionized water and dissolved and stirred for 4h. The obtained solution was slowly added dropwise to solution C. After the addition was completed, stirring was continued for 2h. Under stirring at 70℃, a precipitant of 0.5mol / l (NH4)2CO3 and an equal volume of ammonia water was slowly added dropwise at 3ml / min until the pH was 13, and stirring was continued for 2h. The solution was transferred to a hydrothermal autoclave with an inner liner and crystallized for 12h at 80℃. After crystallization, the solution was centrifuged and washed several times, and then washed with anhydrous ethanol for 3 times. The solution was vacuum dried at 80℃ for 48h to obtain a solid solution superacid precursor. The superacid precursor was calcined at 500℃ in an air atmosphere for 6h to obtain a solid solution superacid catalyst WOx / ZnOZrO2.
[0093] Reaction evaluation:
[0094] The catalyst and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of the catalyst was 1.0g, the mass of the isobutylene was 20.0g, and the mass ratio of the catalyst to the isobutylene was 1:20.
[0095] Comparative Example 4
[0096] Catalyst preparation:
[0097] Weigh 4.46g Zn(NO3)2·6H2O, 18.24g Zr(NO3)4·5H2O was added to 100ml of deionized water and stirred to dissolve to obtain solution A; 1.32g of ammonium metatungstate was weighed and added to 50ml of deionized water and stirred to dissolve to obtain solution B; solution B was slowly added dropwise to solution A under stirring to obtain solution C; a precipitant of equal volumes of 0.5mol / l (NH4)2CO3 and ammonia water was slowly added dropwise at 3ml / min at 70°C with stirring until the pH value was 8.0, and stirring was continued for 2h; the solution was transferred to a hydrothermal autoclave with an inner liner and crystallized for 12h in an environment of 80°C; after crystallization, it was centrifuged and washed several times, and then washed with anhydrous ethanol for 3 times; vacuum dried at 80°C for 48h to obtain a solid solution superacid precursor; the superacid precursor was calcined at 500°C in an air atmosphere for 6h to obtain a solid solution superacid catalyst WOx / ZnOZrO2.
[0098] Reaction evaluation:
[0099] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0100] Comparative Example 5
[0101] Catalyst preparation:
[0102] Weigh 25.59g Zn(NO3)2·6H2O, add 100ml deionized water, stir and dissolve to obtain solution A; weigh 1.32g ammonium metatungstate, add 50ml deionized water, stir and dissolve to obtain solution B; slowly add solution B to solution A under stirring, and obtain solution C after the addition is complete; weigh 10.24g template agent CTAB and 12.60g Tween 40 were added with 100mL deionized water and dissolved and stirred for 4h. The obtained solution was slowly added dropwise to solution C. After the addition was completed, stirring was continued for 2h. Under stirring at 70℃, a precipitant of 0.5mol / l (NH4)2CO3 and an equal volume of ammonia water was slowly added dropwise at 3ml / min until the pH was 8.0, and stirring was continued for 2h. The solution was transferred to a hydrothermal autoclave with an inner liner and crystallized for 12h at 80℃. After crystallization, the solution was centrifuged and washed several times, and then washed with anhydrous ethanol for 3 times. The solution was vacuum dried at 80℃ for 48h to obtain a solid solution superacid precursor. The superacid precursor was calcined at 500℃ in an air atmosphere for 6h to obtain a solid solution superacid catalyst WOx / ZnO.
[0103] Reaction evaluation:
[0104] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0105] Comparative Example 6
[0106] Weigh 24.39g Zr(NO3)4·5H2O, add 100ml deionized water, stir and dissolve to obtain solution A; weigh 1.32g ammonium metatungstate, add 50ml deionized water, stir and dissolve to obtain solution B; slowly drop solution B into solution A under stirring, and obtain solution C after the dropwise addition; weigh 6.56g template agent CTAB and 7.56g Tween 40 were added into 100mL deionized water and dissolved and stirred for 4h. The obtained solution was slowly added dropwise into solution C. After the addition was completed, stirring was continued for 2h. Under stirring at 70℃, a precipitant of 0.5mol / l (NH4)2CO3 and an equal volume of ammonia water was slowly added dropwise at 3ml / min until the pH reached 8.0, and stirring was continued for 2h. The solution was transferred to a hydrothermal autoclave with an inner liner and crystallized for 12h at 80℃. After crystallization, the solution was centrifuged and washed several times, and then washed with anhydrous ethanol for 3 times. The solution was vacuum dried at 80℃ for 48h to obtain a solid solution superacid precursor. The superacid precursor was calcined at 500℃ in an air atmosphere for 6h to obtain a solid solution superacid catalyst WOx / ZrO2.
[0107] Reaction evaluation:
[0108] The catalyst, tert-butanol and liquid isobutylene were put into a reactor, and diisobutylene was synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol was 0.2g, the mass of the catalyst was 1.0g, the mass of isobutylene was 20.0g, and the mass ratio of the catalyst to isobutylene was 1:20.
[0109] Comparative Example 7
[0110] Using Hβ (silicon-aluminum ratio of 100) as a catalyst, the catalyst, tert-butanol and liquid isobutylene are put into a reactor, and diisobutylene is synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol is 0.2g, the mass of the catalyst is 1.0g, the mass of isobutylene is 20.0g, and the mass ratio of the catalyst to isobutylene is 1:20.
[0111] Comparative Example 8
[0112] Using HY (silicon-aluminum ratio 30) as catalyst, the catalyst, tert-butanol and liquid isobutylene are put into a reactor, and diisobutylene is synthesized at a temperature of 70°C, a reaction time of 2h, a nitrogen pressure of 2.0MPa, and a stirring rate of 800rpm; wherein the mass of tert-butanol is 0.2g, the mass of the catalyst is 1.0g, the mass of isobutylene is 20.0g, and the mass ratio of the catalyst to isobutylene is 1:20.
[0113] The diisobutylene prepared in Examples 1-9 and Comparative Examples 1-8 was analyzed, and the analysis standard was based on conventional experiments and regulations in the field. The specific results are shown in Table 1, where:
[0114] Isobutylene conversion calculation:
[0115] Conversion rate = (n 进 -n 出 ) / n 进 *100%;n 进 、n 出 represents the molar amount of imported and exported isobutylene;
[0116] Calculation of diisobutylene selectivity:
[0117] Selectivity = n DIB / (n 进 -n 出 )*100%;n DIB represents the molar amount of diisobutylene.
[0118] Table 1. Performance of catalysts prepared in Examples 1-9 and Comparative Examples 1-8 for catalytic synthesis of diisobutylene
[0119] Implementation catalyst Isobutylene conversion % Diisobutylene selectivity % Example 1 <![CDATA[WOx / ZnOZrO2]]> 93.8 63.4 Example 2 <![CDATA[Ga-WOx / ZnOZrO2]]> 83.6 80.6 Example 3 <![CDATA[La-WOx / ZnOZrO2]]> 85.0 82.5 Example 4 <![CDATA[Sn-WOx / ZnOZrO2]]> 83.3 85.3 Example 5 <![CDATA[Nb-WOx / ZnOZrO2]]> 88.4 83.8 Example 6 <![CDATA[Nd-WOx / ZnOZrO2]]> 82.9 86.5 Example 7 <![CDATA[Al-WOx / ZnOZrO2]]> 89.3 90.4 Example 8 <![CDATA[Ni-WOx / ZnOZrO2]]> 87.1 86.3 Example 9 <![CDATA[La-Al-WOx / ZnOZrO2]]> 90.3 95.2 Comparative Example 1 <![CDATA[ZnOZrO2]]> 4.6 98.7 Comparative Example 2 <![CDATA[WO X / ZnOZrO2(ip)]]> 92.6 44.8 Comparative Example 3 <![CDATA[WOx / ZnOZrO2]]> 65.4 53.0 Comparative Example 4 <![CDATA[WOx / ZnOZrO2]]> 74.5 48.7 Comparative Example 5 <![CDATA[WO X / ZnO]]> 95.5 35.4 Comparative Example 6 <![CDATA[WO X / ZrO2]]> 93.6 22.7 Comparative Example 7 Hβ 94.4 43.4 Comparative Example 8 HY 93.5 38.1
[0120] From the results in Table 1, it can be seen that, compared with the comparative example, the catalyst of the present invention not only improves the conversion rate of diisobutylene but also improves the selectivity of diisobutylene, and the reaction is milder, greener and more economical.
[0121] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A M-WOxZnOZrO2 solid solution superacid catalyst, characterized in that: M is one or more of La, Nd, Nb, Sn, Ga, Al, and Ni; Based on the mass of ZnOZrO2 solid solution, the WOx content is 0.1-30%, the M content is 0.1-20%, and the molar ratio of ZnO to ZrO2 is 10:1-1:20; The preparation method of the M-WOxZnOZrO2 solid solution superacid catalyst comprises the following steps: 1) Weigh a soluble salt of Zn, a soluble salt of Zr and a soluble salt of M, add deionized water and stir to dissolve, to obtain a solution A; 2) Weigh W soluble salt, add deionized water and stir to dissolve, to obtain solution B; 3) Slowly add solution B to solution A under stirring to obtain solution C after the addition is complete; 4) Weigh a certain amount of template, add deionized water, stir for 2-6 hours, slowly drop the obtained solution into solution C, and continue stirring for 2-6 hours after the dropwise addition is completed; the template is CTAB and Tween, and the ratio of the total molar number of the template to the metal ion is 1:1-1:20; 5) slowly adding a precipitant to the solution obtained in step 4) under stirring at 40-90° C. until the pH is 7-12, and continuing stirring for 1-8 hours; 6) transferring the solution obtained in 5) to a hydrothermal reactor and crystallizing at 60-180° C. for 6-48 hours; 7) After crystallization, centrifuge and wash, then wash with anhydrous ethanol for 1-5 times, and vacuum dry to obtain a superacid precursor; 8) The superacid precursor is calcined at 300-1000° C. in an air atmosphere for 2-12 h to obtain a M-WOxZnOZrO2 solid solution superacid catalyst.
2. The M-WOxZnOZrO2 solid solution superacid catalyst according to claim 1, characterized in that: In step 5), the precipitant is one or more of NH4HCO3, (NH4)2CO3, Na2CO3, NaOH, ammonia water or urea, and the dropping speed is 1-5 ml / min.
3. The M-WOxZnOZrO2 solid solution superacid catalyst according to claim 1, characterized in that: In step 6), the crystallization temperature is 70-100° C. and the crystallization time is 6-24 h; in step 7), the vacuum drying temperature is 50-80° C. and the vacuum drying time is 24-48 h.
4. The M-WOxZnOZrO2 solid solution superacid catalyst according to claim 1, characterized in that: In step 8), the calcination temperature is 400-600° C. and the calcination time is 4-10 h.
5. A method for preparing diisobutylene by polymerizing isobutylene, characterized in that: The M-WOxZnOZrO2 solid solution superacid catalyst described in any one of claims 1 to 3 is used to catalyze the reaction of isobutylene in a reactor / fixed bed to prepare diisobutylene.
6. The method according to claim 5, characterized in that The reaction temperature is 40-100° C., the reaction pressure is 0.1-5.0 MPa, the reaction time is 2-10 h, and the mass ratio of the catalyst to isobutylene is 1:10-1:
100.
7. The method according to claim 5, characterized in that During the reaction, one or more of the polar substances methanol, tert-butyl alcohol and MTBE are added as inhibitors, and the mass ratio of the inhibitor to isobutylene is 1:20-1:200.
Citation Information
Patent Citations
Method for the production of diisobutene
CN104395265A
A method for preparing diisobutylene catalyzed by a carbon nanotube-supported ionic liquid catalyst
CN104815695B
Preparation method and equipment of diisobutene or triisobutene
CN1087616A
Selective isobutene dimerizing process to prepare isooctene
CN1810742A
Device of isobutene polymerization preparation diisobutylene , three isobutenes and four isobutenes
CN206622082U