Preparation method and application of cobalt / nitrogen-carbon composite material with double carbon layer
By stirring at room temperature to prepare a cobalt-zinc bimetallic organic framework, and mixing and calcining it with melamine to prepare a double-carbon layer cobalt/nitrogen-carbon composite material, the problem of agglomeration and instability of traditional MOFs during the catalytic process was solved, and sulfamethoxazole was achieved. The efficient removal of azole reduces treatment costs and environmental impact.
Patent Information
- Application Number
- CN202310079364.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-01-29
AI Technical Summary
Traditional wastewater treatment technology has low removal efficiency for sulfamethoxazole (SMX), and metal organic framework materials (MOFs) have agglomeration and instability during the catalytic process, and the solvents used in the synthesis process are not environmentally friendly and require high temperatures. High pressure conditions.
The cobalt-zinc bimetallic organic framework is prepared using a room temperature stirring method, and is mechanically mixed with melamine and calcined to prepare a cobalt/nitrogen-carbon composite material with a double carbon layer to avoid the agglomeration of cobalt nanoparticles. Gradient temperature carbonization is performed in an inert atmosphere to form a stable Cobalt/nitrogen carbon composites.
It achieves efficient removal of emerging pollutants, reduces time and economic costs, and the material is stable, suitable for surface water and groundwater treatment, and has good potential and advantages.
Smart Images

Figure CN116174005B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano materials and removal of new pollutants in wastewater, and in particular to a preparation method and application of a cobalt / nitrogen-carbon composite material with a double carbon layer. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] As one of the most important medical discoveries of the 20th century, antibiotics play an important role in human medicine and aquaculture. However, the abuse and unregulated discharge of antibiotics have led to the generation, proliferation and spread of drug-resistant bacteria and antibiotic resistance genes in the environment, which has not only caused a crisis in the use of antibiotics, but also the emergence of "super-resistant bacteria" has once again seriously threatened human health. In recent years, antibiotic pollution has also attracted great attention from the country and has been included in the national strategy. In order to effectively prevent and control the environmental pollution caused by new pollutants such as persistent organic pollutants, endocrine disruptors and antibiotics that are widely concerned by international conventions at home and abroad. Among the many antibiotics, sulfonamides have been identified as the most commonly used antibiotics in animal husbandry, especially sulfamethoxazole (SMX), which is frequently detected in aquaculture wastewater. However, due to the inherent antibacterial properties and stubbornness of SMX, the removal efficiency of SMX by traditional wastewater treatment technology is low. Therefore, developing an effective SMX degradation method is a feasible strategy to reduce the environmental risk of SMX. Permonosulfate (PMS) advanced oxidation technology is widely used to remove stubborn organic pollutants because it can generate sulfate radicals with strong oxidizing ability and has a wider pH range.
[0004] Among the numerous persulfate catalysts, metal organic framework materials (MOFs) are widely used in the activation of persulfate to remove organic pollutants because of their large specific surface area, high porosity, rich functional groups, and the advantages of adjustable pore size and structure and replaceable functional groups. However, the pore size of most MOFs is in the microporous region, which will greatly limit the diffusion of macromolecules in the porous material. In humid air, aqueous solution or high temperature, some MOFs will even collapse and decompose. Therefore, the inherent instability and microporous structure of MOFs limit their further application in pollutant removal. Research results show that converting traditional bulk MOFs crystals into two-dimensional nanosheets can significantly improve the catalytic performance. This is because two-dimensional nanomaterials have a higher proportion of exposed active atoms to ensure higher catalytic activity, and large nanometer thickness to ensure rapid mass transfer and charge transfer during the reaction. At the same time, pyrolysis of MOFs can optimize the distribution and uniformity of pore size, so the derived carbon materials generally have higher porosity, uniform and adjustable pore size and dispersed active sites. In addition, adjusting the thermal decomposition temperature of MOFs precursors can control the morphology of derived carbon composites. Therefore, MOFs-derived carbon materials have recently attracted widespread attention in the removal of new pollutants by persulfate activation. However, during the pyrolysis of MOFs, metal particles tend to agglomerate. During the synthesis process, a large amount of metal is embedded in the carbon substrate or microporous channels, and loses its function during the catalytic process due to mass transfer limitations. In addition, most MOFs synthesis processes usually use volatile and toxic methanol and N,N-dimethylformamide as solvents, which are not environmentally friendly. At the same time, the preparation process also requires long-term preparation under high temperature and pressure, which is both unsafe and time-consuming. Summary of the invention
[0005] In order to solve the deficiencies of the prior art, the purpose of the present invention is to provide a method for preparing a cobalt / nitrogen-carbon composite material with a double carbon layer and its application. The present invention uses water as a solvent to react and prepare a cobalt-zinc bimetallic organic framework under stirring at room temperature, and then mechanically mixes it with melamine to prepare a precursor of a derived carbon material, and prepares a cobalt / nitrogen-carbon composite material with a double carbon layer by calcination. The present invention can provide a new idea for the preparation of MOFs-derived cobalt-carbon composite materials, and can also open up new ways for the application of MOFs-derived carbon-loaded metal catalysts in pollutant degradation.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing a cobalt / nitrogen-carbon composite material having a double carbon layer, comprising the following steps:
[0008] S1, dropping an aqueous solution of cobalt salt, zinc salt and hexadecyltrimethylammonium bromide into an aqueous solution of 2-methylimidazole, stirring, centrifuging, washing and drying to obtain CoZn-ZIF;
[0009] S2, mixing and grinding CoZn-ZIF and melamine to obtain a mixture;
[0010] S3. Placing the mixture in a tubular furnace under the protection of an inert atmosphere and carbonizing by gradient heating to obtain a cobalt / nitrogen-carbon composite material having a double carbon layer.
[0011] In a second aspect, the present invention provides a cobalt / nitrogen-carbon composite material having a double carbon layer, which is obtained by the preparation method of the cobalt / nitrogen-carbon composite material having a double carbon layer described in the first aspect.
[0012] In a third aspect, the present invention provides use of the cobalt / nitrogen-carbon composite material with a double carbon layer described in the second aspect in removing pollutants.
[0013] The beneficial effects achieved by one or more technical solutions of the present invention are as follows:
[0014] (1) The preparation method of a cobalt / nitrogen-carbon composite material with a double carbon layer provided by the present invention can effectively solve the agglomeration problem of cobalt nanoparticles during the pyrolysis process. The prepared cobalt / nitrogen-carbon composite material with a double carbon layer has a good treatment effect on new pollutants and can be directly put into wastewater for use, thereby reducing time and economic costs.
[0015] (2) The cobalt / nitrogen-carbon composite material with a double carbon layer requires only a very small amount of material to be added when degrading emerging pollutants, and has the advantages of simple operation, low cost, and low energy consumption. It can effectively remove emerging pollutants in surface water and groundwater, and has good potential and advantages in practical engineering applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0017] Figure 1 XRD patterns of Co-N@NC prepared in Example 1 of the present invention, Co@NC prepared in Comparative Example 1, N@NC prepared in Comparative Example 2, and NC prepared in Comparative Example 3;
[0018] Figure 2 This is a transmission electron microscope (TEM) image of Co-N@NC prepared in Example 1 of the present invention;
[0019] Figure 3This is the large-angle annular dark-field spherical aberration electron microscope energy dispersion X-ray elemental spectrum of Co-N@NC prepared in Example 1 of the present invention;
[0020] Figure 4 (a) is a comparison chart of the catalytic effects of removing sulfamethoxazole from persulfate by adding no catalyst group (PMS alone), adding Co-N@NC prepared in Example 1 as a catalyst (Co-N@NC+PMS), adding Co@NC prepared in Comparative Example 1 as a catalyst (Co@NC+PMS), adding N@NC prepared in Comparative Example 2 as a catalyst (N@NC+PMS), and adding NC prepared in Comparative Example 3 as a catalyst (NC+PMS); (b) is a comparison chart of the catalytic effects of Co-N@NC, Co-N@NC-2, Co-N@NC-5 and Co-N@NC-10 prepared in Examples 1-4 of the present invention on removing sulfamethoxazole from persulfate; C t / C0 represents the ratio of the concentration at different reaction times to the initial concentration;
[0021] Figure 5 This is a comparison of the effects of Co-N@NC prepared in Example 1 of the present invention on the degradation of sulfamethoxazole by peroxymonosulfate at different pH values, C t / C0 represents the ratio of the concentration at different reaction times to the initial concentration;
[0022] Figure 6 1 is the XRD spectrum of Co-N@NC prepared in Example 1 of the present invention before and after catalyzing peroxymonosulfate to remove sulfamethoxazole. DETAILED DESCRIPTION
[0023] A first typical embodiment of the present invention is a method for preparing a cobalt / nitrogen-carbon composite material having a double carbon layer, comprising the following steps:
[0024] S1, dropping an aqueous solution of cobalt salt, zinc salt and hexadecyltrimethylammonium bromide (CTAB) into an aqueous solution of 2-methylimidazole, stirring, centrifuging, washing and drying to obtain CoZn-ZIF;
[0025] S2, mixing and grinding CoZn-ZIF and melamine to obtain a mixture;
[0026] S3. Placing the mixture in a tubular furnace under the protection of an inert atmosphere and carbonizing by gradient heating to obtain a cobalt / nitrogen-carbon composite material having a double carbon layer.
[0027] In one or more examples of this embodiment, the cobalt salt in step S1 is one of cobalt chloride, cobalt nitrate, and cobalt sulfate, the zinc salt is one of zinc chloride, zinc sulfate, and zinc nitrate, the molar ratio of the cobalt salt to the zinc salt is 1:15-20, and the molar amount of the cobalt salt is 0.1-0.2 mmol;
[0028] The molar amount of the hexadecyltrimethylammonium bromide is 0.027-0.03 mmol;
[0029] The molar ratio of the 2-methylimidazole to the cobalt salt is 300-500:1.
[0030] In one or more examples of this embodiment, the stirring time in step S1 is 1.5 to 2.5 h, the stirring temperature is room temperature, and the stirring rate is 400 to 600 rpm;
[0031] The washing was performed using methanol.
[0032] In one or more examples of this embodiment, the mass ratio of CoZn-ZIF to melamine in step S2 is 1:1-10.
[0033] In one or more examples of this embodiment, the inert atmosphere in step S3 is one of argon or nitrogen;
[0034] The gradient temperature rise calcination procedure is: firstly, the temperature is raised to 500-600°C at a heating rate of 10°C / min, and kept at that temperature for 1-2h, and then the temperature is raised to 900-1000°C at a heating rate of 5°C / min, and kept at that temperature for 2-3h.
[0035] Since Zn can be reduced to metallic Zn by the supporting carbon material at high temperature, and the boiling point of metallic Zn (908°C) is low, the Zn species evaporates at around 900°C, and the introduction of Co will also promote the evaporation of Zn. Therefore, the introduction of Zn can form a molecular fence effect, increase the distance between Co atoms, and thus inhibit the agglomeration of Co during the calcination process. Melamine can produce ammonia during the calcination process, which will facilitate the migration of Co nanoparticles to the surface of the derived carbon material, thereby exposing more active sites. Since ammonia is generated in situ and is closely adjacent to the metal, it is easier to reduce the metal, and the reduction products are only water and nitrogen, which reduces pollution.
[0036] A second typical embodiment of the present invention is a cobalt / nitrogen-carbon composite material with a double carbon layer, which is obtained by the preparation method of the cobalt / nitrogen-carbon composite material with a double carbon layer described in the first typical embodiment of the present invention.
[0037] In one or more examples of this embodiment, the inner carbon layer of the cobalt / nitrogen-carbon composite material with a double carbon layer is CoZn-ZIF derived carbon, the outer carbon layer is a melamine derived carbon layer, and the cobalt is dispersed in the form of nanoparticles or nanoclusters.
[0038] The third typical embodiment of the present invention is the use of the cobalt / nitrogen-carbon composite material with a double carbon layer described in the second typical embodiment of the present invention in removing pollutants, wherein the application includes activating peroxymonosulfate to remove the new pollutant sulfamethoxazole in wastewater.
[0039] In one or more examples of this embodiment, activating peroxymonosulfate to remove the new pollutant sulfamethoxazole in wastewater comprises the following steps:
[0040] Prepare sulfamethoxazole solution and adjust the pH to 3-11;
[0041] The cobalt / nitrogen-carbon composite material with a double carbon layer according to the second typical embodiment of the present invention is put into a sulfamethoxazole solution, followed by adding peroxymonosulfate to carry out a reaction;
[0042] At specific time intervals, 1 mL of the mixed solution was taken out from the beaker and filtered through a 0.22 μm polytetrafluoroethylene filter into 0.5 mL of methanol to quench the reaction. The mixture was then transferred to a liquid phase vial and the SMX concentration was detected by high performance liquid chromatography.
[0043] In one or more examples of this embodiment, the concentration of sulfamethoxazole in the sulfamethoxazole solution is 10 to 40 mg / L;
[0044] The reaction is carried out in a constant temperature water bath at 15-35° C. with mechanical stirring at 300-500 rpm;
[0045] The input amount of the cobalt / nitrogen-carbon composite material with a double carbon layer is 0.01-0.03 g, and the concentration of the peroxymonosulfate is 0.05-0.2 g / L.
[0046] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.
[0047] Example 1
[0048] 0.0437 g Co(NO3)2·6H2O, 0.8478 g Zn(NO3)2·6H2O and 10 mg CTAB were weighed and dissolved in 20 mL water, 4.9263 g 2-methylimidazole was weighed and dissolved in 130 mL water, and the mixed aqueous solution of Co(NO3)2·6H2O, Zn(NO3)2·6H2O and CTAB was dropped into the 2-methylimidazole aqueous solution under stirring at 500 rpm at room temperature. After stirring for 2 h, the mixture was washed three times by centrifugation with methanol and dried at 60 °C for 12 h to obtain CoZn-ZIF;
[0049] The CoZn-ZIF and melamine were mixed and ground in a mass ratio of 1:1 to obtain a mixture of CoZn-ZIF and melamine;
[0050] The mixture was placed in a tubular furnace under argon protection, first heated to 550°C at a rate of 10°C / min, kept warm for 1 hour, then continued to heat to 1000°C at a rate of 5°C / min, kept warm for 2.5 hours, and the obtained cobalt / nitrogen-carbon composite material with a double carbon layer was recorded as Co-N@NC.
[0051] Example 2
[0052] Different from Example 1, CoZn-ZIF and melamine were mixed and ground in a mass ratio of 1:2, and the finally obtained cobalt / nitrogen-carbon composite material with a double carbon layer was recorded as Co-N@NC-2.
[0053] Example 3
[0054] Different from Example 1, CoZn-ZIF and melamine were mixed and ground in a mass ratio of 1:5, and the finally obtained cobalt / nitrogen-carbon composite material with a double carbon layer was recorded as Co-N@NC-5.
[0055] Example 4
[0056] Different from Example 1, CoZn-ZIF and melamine were mixed and ground in a mass ratio of 1:10, and the finally obtained cobalt / nitrogen-carbon composite material with a double carbon layer was recorded as Co-N@NC-10.
[0057] Comparative Example 1
[0058] Different from Example 1, melamine was not added, and a single layer of nitrogen-doped carbon loaded with cobalt was obtained, which was recorded as Co@NC.
[0059] Comparative Example 2
[0060] Different from Example 1, Co(NO3)2·6H2O is not added, and double carbon layer nitrogen-doped carbon is obtained, which is denoted as N@NC.
[0061] Comparative Example 3
[0062] Different from Example 1, melamine and Co(NO3)2·6H2O were not added, and a single layer of nitrogen-doped carbon was obtained, which was recorded as NC.
[0063] First, the Co-N@NC, Co@NC, N@NC and NC prepared above were characterized by X-ray powder diffraction (XRD). Figure 1As shown, in all samples, there are two diffraction peaks at ~25° and ~44.5°, which can be attributed to the (002) and (101) crystal planes of graphite carbon, respectively. Three diffraction peaks of metallic cobalt phase can be found in Co-N@NC, belonging to the (111), (200) and (220) crystal planes, respectively. However, due to the poor carbon coating and cobalt migration effects, the three diffraction peaks were not found in the XRD spectrum of Co@NC. In order to further verify that the Co-N@NC materials were successfully prepared. The morphology and composition element results of the synthesized Co-N@NC samples are shown in Figure 2 and 3 shown. Figure 2 It is shown that there is no self-aggregation of Co nanoparticles in the transmission electron microscopy (TEM) image of Co-N@NC, which is attributed to the large specific surface area of NC and the rich cobalt loading sites it provides. At the same time, it can be found that the edge of the material includes a double carbon layer, the inner carbon layer is attributed to MOF-derived carbon, and the outer carbon layer is attributed to melamine-derived carbon layer. The presence of graphite carbon layer can promote electron transfer in the pollutant removal process. High-angle annular dark field spherical aberration electron microscopy energy dispersive X-ray elemental map of Co-N@NC (HAADF-STEM-EDX-Map1ngs, Figure 3 ) showed that C and N elements were regularly dispersed on the surface of the material. Co element was dispersed throughout the material in the form of Co nanoparticles and a small amount of Co clusters. The above results prove that the cobalt / nitrogen-carbon composite material with double carbon layer was successfully prepared.
[0064] Example 5
[0065] The SMX removal experiment process is as follows: first take 200mL of prepared SMX with an initial pH of 7.08 in a 250mL beaker. Then, place the beaker in a constant temperature water bath, keep the temperature at 25°C, and add 20mg of catalyst and 20mg of PMS to the SMX solution in sequence while stirring at a stirring rate of 400rpm, and the reaction starts immediately. Take out 1mL of the mixed solution from the beaker at specific time intervals, filter it through a 0.22μm polytetrafluoroethylene filter membrane into 0.5mL of methanol, quench the termination reaction, and then transfer it to a liquid phase vial, and detect the SMX concentration by high performance liquid chromatography. In the above scheme, the high performance liquid phase analysis uses a Thermo HPLC system. Detector: UV lamp; chromatographic column: BDS HYPERSIL.C18, 150×4.6 mm; flow rate: 1 mL / min; mobile phase: acetonitrile / water (containing 0.2% formic acid) = 40 / 60 (v / v); injection volume: 10 μL; column temperature: 35°C; detection wavelength: 270 nm.
[0066] from Figure 4a It can be seen that under the condition of an initial pH of 7.08, the 120-min removal rate of SMX by PMS alone was 28.46%. Within 120 minutes, the degradation effects of Co@NC (41.48%) and Co-N@NC (97.09%) on SMX were better than those of NC (31.07%) and N@NC (28.02%). The results show that the addition of Co enhances the ability of NC and N@NC to catalyze PMS. At the same time, it is also proved that cobalt nanoparticles are the main active sites for catalyzing the degradation of SMX by PMS. Compared with Co@NC, Co-N@NC not only showed the highest removal rate for SMX, but also showed the best reaction activity. The reason for this is that the addition of melamine produces ammonia in situ during the calcination process, and ammonia promotes the migration of more cobalt nanoparticles to the surface of the derived carbon, exposing the active sites with a greater probability, thereby enhancing the degradation effect of SMX. In addition, further increasing the mass ratio of melamine and cobalt-zinc MOF precursor does not further promote the degradation of SMX ( Figure 4 b) The reason is that the cobalt nanoparticles have reached the maximum exposure ratio at a mass ratio of 1:1, and there is no difference in the cobalt content, so the exposed cobalt sites will not increase further, and therefore the SMX degradation effect will not be further enhanced.
[0067] like Figure 5 As shown. After 120 minutes of reaction, under the condition of initial pH of 3.48-9.25, the degradation rates of SMX were 96.67, 98.23, 97.09 and 97.88%, respectively. At a pH of 10.71, the degradation efficiency of SMX still reached 59.35%. The results show that Co-N@NC not only has good catalytic activity but also has a wide pH range of application. In addition, the pH of organic wastewater is usually close to neutral, so the material prepared by the present invention has good potential for efficient treatment of actual wastewater.
[0068] In order to explore the stability of Co-N@NC, the reacted Co-N@NC was washed with ethanol and ultrapure water by centrifugation and dried, and then characterized by XRD. Figure 6 As shown in Figure 2, no oxidation state of Co was observed in the XRD spectrum of Co-N@NC after the reaction. The results show that Co-N@NC has good stability.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. Application of a cobalt / nitrogen-carbon composite material having a double carbon layer in removing new pollutants, characterized in that: The applications include activating peroxymonosulfate to remove sulfamethoxazole, a new pollutant in wastewater; The activated peroxymonosulfate to remove the new pollutant sulfamethoxazole in wastewater comprises the following steps: Prepare sulfamethoxazole solution and adjust the pH to 3 ~ 11; The cobalt / nitrogen-carbon composite material having a double carbon layer is put into a sulfamethoxazole solution, followed by the addition of peroxymonosulfate to carry out a reaction; At specific time intervals, 1 mL of the mixed solution was taken out from the beaker and filtered through a 0.22 μm polytetrafluoroethylene filter into 0.5 mL of methanol to quench the reaction, and then transferred to a liquid phase vial, and the SMX concentration was detected by high performance liquid chromatography; The inner carbon layer of the cobalt / nitrogen-carbon composite material with double carbon layers is CoZn-ZIF derived carbon, the outer carbon layer is a melamine derived carbon layer, and the cobalt is dispersed in the form of nanoparticles or nanoclusters; The method for preparing the cobalt / nitrogen-carbon composite material having a double carbon layer comprises the following steps: S1, dropping an aqueous solution of cobalt salt, zinc salt and hexadecyltrimethylammonium bromide into an aqueous solution of 2-methylimidazole, stirring, centrifuging, washing and drying to obtain CoZn-ZIF; S2, mixing and grinding CoZn-ZIF and melamine to obtain a mixture; S3, placing the mixture in a tube furnace under the protection of an inert atmosphere, and carbonizing by gradient heating to obtain a cobalt / nitrogen-carbon composite material having a double carbon layer; In step S2, the mass ratio of CoZn-ZIF to melamine is 1:1 to 10.
2. The use according to claim 1, characterized in that The sulfamethoxazole concentration in the sulfamethoxazole solution is 10 to 40 mg / L; The reaction is carried out under mechanical stirring at 300-500 rpm and in a constant temperature water bath at 15-35°C; the input amount of the cobalt / nitrogen-carbon composite material with a double carbon layer is 0.01-0.03 g, and the concentration of peroxymonosulfate is 0.05-0.2 g / L.
3. The use according to claim 1, characterized in that In step S1, the cobalt salt is one of cobalt chloride, cobalt nitrate, and cobalt sulfate, the zinc salt is one of zinc chloride, zinc sulfate, and zinc nitrate, the molar ratio of the cobalt salt to the zinc salt is 1:15 to 20, and the molar amount of the cobalt salt is 0.1 to 0.2 mmol; The molar amount of the hexadecyltrimethylammonium bromide is 0.027 to 0.03 mmol; The molar ratio of the 2-methylimidazole to the cobalt salt is 300 to 500:
1.
4. The use according to claim 1, characterized in that In step S1, the stirring time is 1.5 to 2.5 h, the stirring temperature is room temperature, and the stirring rate is 400 to 600 rpm; The washing was performed using methanol.
5. The method for preparing the cobalt / nitrogen-carbon composite material having a double carbon layer according to claim 1, characterized in that: The inert atmosphere in step S3 is one of argon or nitrogen; The gradient temperature rise calcination procedure is: firstly increase the temperature to 500-600°C at a heating rate of 10°C / min, keep it warm for 1-2 hours, then continue to increase the temperature to 900-1000°C at a heating rate of 5°C / min, and keep it warm for 2-3 hours.
Citation Information
Patent Citations
MOFs-based cobalt / nitrogen-doped carbon material capable of activating peroxymonosulfate as well as preparation method and application thereof
CN112264082A