Polymers used as additives for fiber optic cable greases

By using structural comb or linear block copolymers in optical cable grease, the problem of compatibility of polar and non-polar components is solved, the compatibility and water resistance of the grease are improved, and better performance is achieved balance.

CN116178638BActive Publication Date: 2024-10-18SHENYANG RES INST OF CHEM IND
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202111420158.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-10-18
Estimated Expiration
2041-11-26

AI Technical Summary

Technical Problem

The compatibility problem between polar and non-polar components in optical cable grease limits the choice of additive types and affects product performance.

Method used

Structural comb-type graft block copolymers or linear block copolymers are used as optical cable ointment additives, through the coagulation of aryl olefins and conjugated diene monomers with alkyl (meth)acrylates or fluoroalkyl esters. Valent linkages form polymers to improve the compatibility and water resistance of the internal components of the ointment.

Benefits of technology

Through the covalent connection of polar and non-polar blocks, it promotes the dispersion of polar additives in the ointment, improves compatibility, and enhances water resistance through the graft structure to achieve a good balance effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003377038670000021
    Figure BDA0003377038670000021
  • Figure BDA0003377038670000022
    Figure BDA0003377038670000022
  • Figure FDA0005026521260000011
    Figure FDA0005026521260000011
Patent Text Reader

Abstract

The present invention relates to the field of anionic active polymers, and further to fillers used in optical cables, and specifically to a polymer used as an additive for optical cable ointment. The polymer is a comb-type graft block copolymer or a linear block copolymer, and the number average molecular weight is 1000-100,000. In the polymer used as an additive for optical cable ointment of the present invention, polymer 2 provides a compatibilizing effect, and through the covalent connection between the polar 2b block and the non-polar and / or weakly polar 2a block, the polar additive component in the ointment is promoted to be dispersed in the non-polar and / or weakly polar ointment body, thereby improving the compatibility of the ointment components and taking into account the effect of water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of anionic active polymers, more particularly to fillers used in optical cables, and more particularly to a polymer used as an additive for optical cable ointment. Background Art

[0002] Optical cable grease is a filler used in optical cables. It mainly plays a role in mechanical buffering and water blocking, and has an important impact on the performance of optical cables. Optical cable grease is composed of base oil, viscosity index improver, gelling agent (thickener), antioxidant and other additives such as preservatives, surfactants, dehydrogenation agents, etc., among which the gelling agent is the key component affecting the performance of the grease. Gelling agents include fatty acid salts, organic bentonite, fumed silica, paraffin, polymers and other options. Among them, polymers have excellent miscibility with base oil and have received more attention. (Optical Fiber and Cable and Its Application Technology, 1994, (6): 38-40; Wire and Cable Materials: Structure, Performance and Application, Beijing: Machinery Industry Press, 2012: 266-267.)

[0003] Among polymer gelling agents, linear hydrogenated styrene-isoprene block copolymers (diblock is denoted as SEP and triblock is denoted as SEPS) prepared by anionic living polymerization are the most influential varieties. Documents CN1875435A, CN1926642A, and CN108864641A reported ointment formulations using styrene-conjugated diene copolymer elastomer as gelling agent; CN107793542B reported a method of adding weak polar solvent toluene to the SEP polymerization system to reduce the oligomer content in the product; CN112708085A reported a star-shaped SEP gelling agent.

[0004] The above-mentioned literature records that a variety of polar and non-polar components are mixed in the optical cable grease, and the compatibility between them becomes an important consideration in selecting the type of additives, thus restricting the selection range of the additive types and affecting the performance of the product. Summary of the invention

[0005] In view of the above problems, the present invention provides a polymer used as an additive for optical cable grease.

[0006] To achieve the above purpose, the present invention adopts the following technical solution:

[0007] A polymer used as an additive for optical cable ointment, wherein the polymer is a comb-type graft block copolymer or a linear block copolymer, and the number average molecular weight is 1000-100,000, preferably 10,000-50,000, and more preferably 10,000-40,000.

[0008] The structural comb-type graft block copolymer is a polymer 1 having the following structure, wherein the polymer 1 is composed of a block 1a formed by graft copolymerization of aromatic olefins and / or conjugated diene monomers and a block 1b formed by polymerization of (meth) fluoroalkyl acrylate, which are covalently connected;

[0009]

[0010] The linear block copolymer is a polymer 2 having the following structure, wherein the polymer 2 is composed of a block 2a formed by polymerization of aromatic olefins and / or conjugated diene monomers and a block 2b formed by polymerization of (meth) alkyl acrylate, which are covalently connected;

[0011]

[0012] The aromatic olefin is one or more of styrene and its derivatives, preferably styrene and methylstyrene, and more preferably styrene;

[0013] The conjugated diene is butadiene (1,3-butadiene) or isoprene (2-methyl-1,3-butadiene);

[0014] The linking units of the covalently connected blocks 1a and 1b, 2a and 2b are ethylenic monomers having steric hindrance and capable of inhibiting the subsequent anionic polymerization side reaction of the (meth)acrylate monomer, and may be any type involved in the prior art, preferably 1,1-diphenylethylene (DPE) and its derivatives, more preferably DPE;

[0015] The (meth) acrylic acid alkyl ester is acrylic acid or methacrylic acid and C1-C 20 Esters of alkyl alcohols;

[0016] The (meth)acrylic acid fluoroalkyl ester is acrylic acid or methacrylic acid and C1-C 20 Esters of fluoroalkyl alcohols.

[0017] Further,

[0018] The aromatic olefin is one or more of styrene, methylstyrene, dimethylstyrene, trimethylstyrene, ethylstyrene, propylstyrene and other styrene derivatives, preferably styrene and methylstyrene, and more preferably styrene.

[0019] The (meth) acrylic acid alkyl ester is acrylic acid or methacrylic acid and C1-C 10 Esters composed of alkyl alcohols; more preferably methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, lauryl (meth)acrylate, etc., and more preferably methyl (meth)acrylate and butyl (meth)acrylate;

[0020] The (meth)acrylic acid fluoroalkyl ester is acrylic acid or methacrylic acid and C1-C 10 Esters composed of fluoroalkyl alcohols, such as trifluoroethyl methacrylate, hexafluorobutyl methacrylate, etc.

[0021] The polymer 1 and polymer 2 are prepared by respectively polymerizing their two blocks through solvent anionic living polymerization.

[0022] The initiator is selected from alkyl lithium, such as n-butyl lithium, sec-butyl lithium, tert-butyl lithium, naphthalene lithium, etc. In the present invention, n-butyl lithium is selected.

[0023] The solvent may be any one or a mixture thereof in the prior art, and is not limited in the present invention. The present invention preferably uses cyclohexane, or a mixture of n-hexane and cyclohexane as the basic component of the solvent. Since the aforementioned solvent components are all non-polar, in order to take into account the solubility of the polar components that may be introduced, a polar solvent may be added as a cosolvent, such as toluene, tetrahydrofuran, etc., any one or a mixture thereof in the prior art, and is not limited in the present invention.

[0024] Preparation of polymer 1: It is necessary to first prepare a macromolecular monomer composed of aromatic olefins and / or conjugated diene monomers. The preparation method can refer to existing literature, such as: Synthetic Rubber Industry, 2015, 38(1): 25-29; Fine Chemicals, 2019, 36(8): 1702-1707. A structure regulator may or may not be used in the preparation process to adjust the microstructure of the polymer; the structure regulator used may be any one or a mixture thereof involved in the prior art, and is not limited in the present invention. The initiator initiates the polymerization of the monomer, which is then capped with a capping agent, and then an end-capping agent is added to cap the end to obtain the desired macromolecular monomer.

[0025] On the basis of the aforementioned macromonomer, the mixture of aromatic olefin and / or conjugated diene monomer and macromonomer is again initiated by an initiator to obtain active species of block 1a; the active species of block 1a is then anion polymerized with (meth) fluoroalkyl acrylate monomer to connect block 1b, and finally terminated with a terminator to obtain polymer 1.

[0026] The terminator can be any type involved in the prior art, such as water, alcohols, hydrogen, etc., preferably isopropanol, and the amount used is more than 1 times the molar amount of the initiator, which is not limited in the present invention.

[0027] Preparation of polymer 2:

[0028] The initiator initiates anionic polymerization of aromatic olefin and / or conjugated diene monomers to obtain active species of block 2a; the active species of block 2a is then anion polymerized with (meth) alkyl acrylate monomers to connect block 2b, and finally terminated with a terminator to obtain polymer 2.

[0029] The anionic polymerization method of the aforementioned blocks 1a to 1b and 2a to 2b can be any method mentioned in the existing literature, which is known to those skilled in the art and is not limited in this scheme. Considering the prospect of large-scale production, a method that can react under relatively mild temperature conditions is preferred, and reference can be made to existing literature, such as: RSC Advances, 2017, 7(16): 9933-9940.

[0030] The invention discloses an application of a polymer, wherein the polymer is used as an additive for filling grease of communication optical cables.

[0031] The polymers are polymer 1 and polymer 2; wherein the added amount of the polymers accounts for 1-60% of the mass of the main agent of the communication optical cable filling paste gelling agent (ie SEP or SEPS), preferably 10-40%.

[0032] The polymers are polymer 1 and polymer 2; wherein the mass ratio of polymer 1 to polymer 2 is 0.01-100, preferably 0.1-50, and more preferably 1-5.

[0033] The advantages and positive effects of the present invention are:

[0034] The polymer 2 in the polymer used as an additive for optical cable ointment of the present invention provides a compatibilizing effect, and through the covalent connection between the polar 2b block and the non-polar and / or weakly polar 2a block, promotes the dispersion of the polar additive component in the ointment in the non-polar and / or weakly polar ointment body, thereby improving the compatibility of the components inside the ointment;

[0035] At the same time, polymer 1 provides water resistance compensation, making up for the disadvantages of increased polar groups and increased hydrophilicity caused by the introduction of polymer 2, and maintaining the water resistance of the ointment. The grafted structure of the 1a block helps to increase the entanglement with the SEP chain segment, the main component of the ointment gelling agent, and alleviates the phase separation defect caused by the incompatibility of the 1b block with the main body of the gelling agent.

[0036] When polymers 1 and 2 work together, a better balance is achieved between improving the compatibility of the internal components of the ointment and maintaining the water resistance of the ointment. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with specific embodiments.

[0038] In the solvent anionic polymerization reaction system, the materials used should be refined in advance according to the prior art to reduce the water and oxygen content to less than 10ppm. The refining method used is known to those skilled in the art and is not limited in this scheme. The reaction vessel used is a 5L stainless steel pressure reactor. During the reaction, the mechanical stirring is kept turned on, with a rotation speed of 1-1000rpm, preferably 300-400rpm. The initiator is a n-butyl lithium hexane solution with a concentration of 1.4-2.5mol / L, and can also be further diluted with a solvent (such as n-hexane). The concentration of the n-butyl lithium hexane solution used in the present invention is 2.5mol / L.

[0039] Example 1-1: Macromonomer for preparing polymer 1

[0040] At a temperature of 51°C, 1355g of cyclohexane and 53g of styrene were added to the reactor. The stirring rate was about 350rpm, and 10.6mL of 2.5mol / L n-butyl lithium hexane solution was added to initiate the reaction for 1h. 10.7g of 1,1-diphenylethylene was added and the reaction was continued for 0.5h. The temperature was lowered to 10°C, and 5g of p-vinylbenzyl chloride dissolved in 25g of tetrahydrofuran was added and the reaction was continued for 1h. After the reaction was completed, the macromolecular monomer product was precipitated with ethanol and washed, and then vacuum dried at 40°C for 12h. The product was analyzed by GPC, and the molecular weight of the obtained polymer was 2.8×10 3 , the distribution width is 1.02.

[0041] Example 1-2: Macromonomer for preparing polymer 1

[0042] At a temperature of 50°C, 928g of cyclohexane, 461g of n-hexane and 41g of styrene were added to the reactor. The stirring rate was about 350rpm, and 11.3mL of 2.5mol / L n-butyl lithium hexane solution was added to initiate the reaction, and the reaction was continued for 1h. 0.6g of tetramethylethylenediamine and 10g of isoprene were added, and the reaction was continued for 1h. 9.9g of 1,1-stilbene was added, and the reaction was continued for 0.5h. The temperature was lowered to 3°C, and 6.1g of p-vinylbenzyl chloride dissolved in 23g of tetrahydrofuran was added, and the reaction was continued for 1h. After the reaction was completed, the macromolecular monomer product was precipitated with ethanol and washed, and then dried in a vacuum at 40°C for 12h. The product was analyzed by GPC, and its molecular weight was 2.7×10 3 , the distribution width is 1.03.

[0043] Examples 1-3: Macromonomers for preparing polymer 1

[0044] At a temperature of 53°C, 1003g of cyclohexane, 266g of n-hexane and 48g of styrene were added to the reactor. The stirring rate was about 350rpm, and 12.7mL of 2.5mol / L n-butyl lithium hexane solution was added to initiate the reaction, and the reaction was continued for 1h. 0.7g of diethylene glycol monomethyl ether and 11g of isoprene were added, and the reaction was continued for 1h. 8.1g of 1,1-stilbene was added, and the reaction was continued for 0.5h. The temperature was lowered to 5°C, and 5.3g of p-vinylbenzyl chloride dissolved in 28g of tetrahydrofuran was added, and the reaction was continued for 1h. After the reaction was completed, the macromolecular monomer product was precipitated with ethanol and washed, and then dried under vacuum at 40°C for 12h. The product was analyzed by GPC, and its molecular weight was 2.7×10 3 , the distribution width is 1.03.

[0045] Example 2-1: Polymer 1

[0046] At a temperature of 44°C, 522g of cyclohexane, 487g of toluene, 226g of n-hexane, and 33g of styrene were added to the reactor. The stirring rate was about 350rpm, and 2.5mL of 2.5mol / L n-butyl lithium hexane solution was added to initiate the reaction, and the reaction was continued for 1h. 10.2g of tetrahydrofuran, 103g of isoprene, and 14.1g of the macromonomer prepared in Example 1-1 pre-dissolved in an appropriate amount of toluene were added, and the reaction was continued for 1h. 4.1g of 1,1-diphenylethylene was added and the reaction was continued for 0.5h. The temperature was lowered to 5°C, and 3.3g of trifluoroethyl methacrylate, 5.2g of hexafluorobutyl methacrylate, and 4.7g of dodecafluoroheptyl acrylate were added and the reaction was continued for 1h. After the reaction was completed, isopropanol was added to terminate the reaction. The hydrogenation and post-treatment were carried out by the methods described in CN111892669A and CN112142883A. The polymer 1 product was precipitated with ethanol and washed. The unreacted macromolecular monomer was removed by reflux washing with acetone and dried in vacuum at 40°C for 12 hours. The product was analyzed by GPC and its molecular weight was 3.4×10 4 , the distribution width is 1.42.

[0047] Example 2-2: Polymer 1

[0048] At a temperature of 52°C, 350g of cyclohexane, 357g of toluene, 528g of n-hexane, and 41g of styrene were added to the reactor. The stirring rate was about 350rpm, and 2.3mL of 2.5mol / L n-butyl lithium hexane solution was added to initiate the reaction, and the reaction was carried out for 1h. 7.9g of tetrahydrofuran, 0.6g of diethylene glycol monomethyl ether, 97g of isoprene, and 14.5g of the macromonomer prepared in Example 1-2 pre-dissolved in toluene were added, and the reaction was carried out for 1h. 3.8g of 1,1-diphenylethylene was added and the reaction was carried out for 0.5h. The temperature was lowered to 6°C, 4.5g of trifluoroethyl acrylate, 6.6g of hexafluorobutyl methacrylate, and 3.6g of dodecafluoroheptyl methacrylate were added, and the reaction was carried out for 1h. After the reaction was completed, isopropanol was added to terminate the reaction. The aforementioned method was used for hydrogenation and post-treatment, and the polymer 1 product was precipitated and washed with ethanol, and the unreacted macromonomer was removed by reflux washing with acetone, and vacuum dried at 40°C for 12h. The product was analyzed by GPC and its molecular weight was 3.3×10 4 , the distribution width is 1.45.

[0049] Example 2-3: Polymer 1

[0050] At a temperature of 57°C, 413g of cyclohexane, 429g of toluene, 433g of n-hexane, and 39g of styrene were added to the reactor. The stirring rate was about 350rpm, and 2.6mL of 2.5mol / L n-butyl lithium hexane solution was added to initiate the reaction, and the reaction was carried out for 1h. 9.3g of tetrahydrofuran, 0.5g of diethylene glycol dimethyl ether, 90g of isoprene, and 13.8g of the macromonomer prepared in Example 1-2 pre-dissolved in toluene were added, and the reaction was carried out for 1h. 4.4g of 1,1-diphenylethylene was added and the reaction was carried out for 0.5h. The temperature was lowered to 1°C, and 5.1g of trifluoroethyl methacrylate, 2.3g of hexafluorobutyl acrylate, and 7.9g of dodecafluoroheptyl methacrylate were added and the reaction was carried out for 1h. After the reaction was completed, isopropanol was added to terminate the reaction. The aforementioned method was used for hydrogenation and post-treatment, and the polymer 1 product was precipitated and washed with ethanol, and the unreacted macromonomer was removed by reflux washing with acetone, and vacuum dried at 40°C for 12h. The product was analyzed by GPC and its molecular weight was 3.6×10 4 , the distribution width is 1.4.

[0051] Example 3-1: Polymer 2

[0052] At a temperature of 47°C, 925g of cyclohexane, 467g of n-hexane and 37g of styrene were added to the reactor. The stirring rate was about 350rpm, and 3.6mL of 2.5mol / L n-butyl lithium hexane solution was added to initiate the reaction for 1h. 12.1g of tetrahydrofuran, 0.9g of tetramethylethylenediamine and 86g of isoprene were added and the reaction was continued for 1h. 5.1g of 1,1-stilbene was added and the reaction was continued for 0.5h. The temperature was lowered to 2°C, 2.1g of methyl methacrylate, 2.3g of butyl acrylate and 5.7g of lauryl methacrylate were added and the reaction was continued for 1h. After the reaction was completed, isopropanol was added to terminate the reaction. The aforementioned method was used for hydrogenation and post-treatment, and the polymer 2 product was precipitated and washed with ethanol and dried in vacuo at 40°C for 12h. The product was analyzed by GPC, and its molecular weight was 2.1×10 4 , the distribution width is 1.46.

[0053] Example 3-2: Polymer 2

[0054] At a temperature of 53°C, 693g of cyclohexane, 634g of n-hexane and 40g of styrene were added to the reactor. The stirring rate was about 350rpm, and 2.9mL of 2.5mol / L n-butyl lithium hexane solution was added to initiate the reaction, and the reaction was carried out for 1h. 11.7g of tetrahydrofuran, 0.7g of diethylene glycol dimethyl ether, and 90g of isoprene were added and reacted for 1h. 6.6g of 1,1-stilbene was added and reacted for 0.5h. The temperature was lowered to 1°C, 3.7g of methyl acrylate, 1.6g of butyl methacrylate, and 7.9g of lauryl methacrylate were added and reacted for 1h. After the reaction was completed, isopropanol was added to terminate the reaction. The aforementioned method was used for hydrogenation and post-treatment, and the polymer 2 product was precipitated with ethanol and washed, and then dried in vacuo at 40°C for 12h. The product was analyzed by GPC, and its molecular weight was 2.5×10 4 , the distribution width is 1.42.

[0055] Example 3-3: Polymer 2

[0056] At a temperature of 50°C, 881g of cyclohexane, 524g of n-hexane and 34g of styrene were added to the reactor. The stirring rate was about 350rpm, and 3.1mL of 2.5mol / L n-butyl lithium hexane solution was added to initiate the reaction for 1h. 10.8g of tetrahydrofuran, 0.6g of diethylene glycol monomethyl ether and 93g of isoprene were added and the reaction was continued for 1h. 7.3g of 1,1-stilbene was added and the reaction was continued for 0.5h. The temperature was lowered to 3°C, 4.1g of methyl methacrylate, 2.2g of butyl methacrylate and 4.8g of lauryl acrylate were added and the reaction was continued for 1h. After the reaction was completed, isopropanol was added to terminate the reaction. The aforementioned method was used for hydrogenation and post-treatment, and the polymer 2 product was precipitated and washed with ethanol and dried in vacuo at 40°C for 12h. The product was analyzed by GPC, and its molecular weight was 2.4×10 4 , the distribution width is 1.39.

[0057] The polymer prepared in the above embodiment is added to the optical cable paste additive, specifically:

[0058] Example 4-1: Formulation Experiment

[0059] At a temperature of 107°C, 120g of polyolefin base oil, 10g of SEP, 2.3g of polymer 1 prepared in Example 2-2, 0.9g of polymer 2 prepared in Example 3-2, and 1.3g of Irganox alkylphenol antioxidant were added to a beaker and mixed evenly. The oil separation value of the steel mesh was measured by the method described in the industry standard SH / T 0324 and was 2.15%.

[0060] Example 4-2: Formulation Experiment

[0061] At a temperature of 122°C, 131 g of polyolefin base oil, 9 g of SEP, 3.5 g of polymer 1 prepared in Example 2-3, 1.3 g of polymer 2 prepared in Example 3-3, and 1.4 g of Irganox alkylphenol antioxidant were added to a beaker and mixed evenly. The oil separation value of the steel mesh was measured by the method described in the industry standard SH / T 0324 and was 1.98%.

[0062] Comparative Example: Formulation Experiment

[0063] At a temperature of 113° C., 117 g of polyolefin base oil, 12 g of SEP, and 1.2 g of Irganox alkylphenol antioxidant were added into a beaker and mixed evenly. The oil separation value of the steel mesh was measured to be 2.36%.

[0064] The water resistance of the above-mentioned Examples 4-1, 4-2 and Comparative Example was measured by the method described in the industry standard SH / T 0453, and no body was found.

[0065] In summary, the present invention improves the compatibility of the internal components of the ointment by adding polymer 1 and polymer 2, while taking into account the water resistance of the ointment, thereby achieving a better effect, and the effect is particularly obvious when the polymers are added in a certain proportion.

[0066] Although the present invention has been described to a certain extent, it is obvious that appropriate changes in various conditions can be made without departing from the spirit and scope of the present invention. It is understood that the present invention is not limited to the embodiments described, but belongs to the scope of the claims, which includes equivalent replacements of each factor described.

Claims

1. A polymer used as an additive for optical cable grease, characterized in that: The polymer is a comb-type graft block copolymer with a number average molecular weight of 1000-100,000; The structural comb-type graft block copolymer is a polymer 1 having the following structure, which is composed of a block 1a formed by graft copolymerization of aromatic olefins and / or conjugated diene monomers and a block 1b formed by polymerization of (meth) fluoroalkyl acrylate, which are covalently connected; 2. The polymer used as an additive for optical cable grease according to claim 1, characterized in that: The aromatic olefin is one or more of styrene and its derivatives; The conjugated diene is butadiene (1,3-butadiene) or isoprene (2-methyl-1,3-butadiene); (Meth) fluoroalkyl acrylate is acrylic acid or methacrylic acid and C1-C 20 Esters of fluoroalkyl alcohols.

3. The polymer used as an additive for optical cable grease according to claim 2, characterized in that: The aromatic olefin is one or more of styrene, methylstyrene, dimethylstyrene, trimethylstyrene, ethylstyrene, propylstyrene and other styrene derivatives; The (meth)acrylic acid fluoroalkyl ester is acrylic acid or methacrylic acid and C1-C 10 Esters of fluoroalkyl alcohols.

4. The polymer used as an additive for optical cable grease according to claim 1, characterized in that: The polymer 1 is prepared by solvent anionic living polymerization.

5. An application of the polymer according to claim 1, characterized in that: Use of the polymer described in claim 1 as an additive for filling paste of communication optical cables.

6. Use of the polymer according to claim 5, characterized in that: The polymer described in claim 1 is polymer 1; the additive further comprises polymer 2; the polymer 2 is composed of a block 2a formed by polymerization of aromatic olefins and / or conjugated diene monomers and a block 2b formed by polymerization of (meth) alkyl acrylate, which are covalently connected; the addition amount of polymer 1 and polymer 2 is 1-60% of the mass of the main agent of the communication optical cable filling paste gelling agent; 7. Use of the polymer according to claim 6, characterized in that: The mass ratio of polymer 1 to polymer 2 is 0.01-100.

Citation Information

Patent Citations

  • A method for synthesizing hydrogenated styrene / isoprene block copolymers

    CN107793542B

  • Optical cable coating material with high bonding strength and preparation method thereof

    CN108864641A

  • Hydrogenated amino functionalized styrene-butadiene rubber and preparation method thereof

    CN111892669A

  • Continuous hydrogenation method and device for conjugated diene polymer

    CN112142883A

  • Hydrogenated isoprene / styrene block coupling polymer optical cable ointment gelling agent, preparation method thereof and application thereof in optical cable ointment

    CN112708085A