Non-metallic B-doped β-phase MnO2 electrode material and its preparation method and application
The hydrothermal preparation of non-metallic boron-doped β-phase MnO2 electrode materials solved the problem of poor cycle stability of β-MnO2 electrode materials in zinc-ion batteries, achieving high specific capacity and long cycle life battery performance, and simplifying the preparation process.
Patent Information
- Application Number
- CN202310055494.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-01-17
AI Technical Summary
Existing β-MnO2 electrode materials have unsatisfactory cycle stability in zinc-ion batteries, mainly due to lattice expansion caused by Zn ion insertion and extraction and Mn ion dissolution.
A method for preparing non-metallic B-doped β-phase MnO2 electrode materials was adopted. The non-metallic B-doped β-phase MnO2 electrode materials were synthesized by hydrothermal method, which enhanced the insertion and extraction ability of Zn ions, improved the conductivity, and inhibited the dissolution of Mn ions.
It improves the specific capacity and cycle stability of aqueous zinc-ion batteries, with a specific capacity retention rate of over 87.96% after 1000 cycles. It also improves conductivity, simplifies the preparation process, and facilitates industrialization.
Smart Images

Figure CN116199264B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of aqueous zinc ion battery energy storage, and specifically relates to an electrode material. More specifically, the present invention relates to a non-metallic B-doped β-phase MnO2 electrode material and a preparation method and application thereof. Background Art
[0002] With the rapid development of society, electricity is indispensable in all aspects of life, and energy storage has become a key technology for electricity applications. At present, lithium-ion batteries are widely used in the field of energy storage, but the safety issues that come with it need to be solved urgently. To this end, we have explored an aqueous zinc-ion battery. This battery system is a high-safety energy storage device based on aqueous electrolytes. It has many advantages such as large specific capacity, high safety, low cost, and green environmental protection. It has become one of the most promising electrochemical energy storage devices.
[0003] The cathode materials of aqueous zinc-ion batteries are mainly divided into manganese-based oxides, vanadium-based oxides, Prussian blue analogs and organic compounds. Due to the high cost and toxicity of vanadium-based oxides, the good rate performance of Prussian blue analogs and organic compounds but low capacity, and the many advantages of manganese-based oxides such as excellent specific capacity, large voltage window, and abundant storage capacity, we have focused on manganese-based oxides.
[0004] MnO2 is a manganese-based oxide that is currently being studied more. MnO2 is generally dominated by +4 valence, but there are a small amount of +2 and +3 ions. Only β-MnO2 can be considered that the valence state of Mn is equal to +4, so the specific capacity is higher than other crystal forms. However, during the battery charging and discharging process, the embedding and extraction of Zn ions in the cathode material causes lattice expansion, and the disproportionation reaction of Mn ions causes partial dissolution of Mn, making the cyclic stability of β-MnO2 not very ideal. In order to improve the cyclic stability of β-MnO2, a non-metallic doping is proposed.
[0005] Based on the above reasons, this application is hereby filed. Summary of the invention
[0006] Based on the above reasons, in view of the problems or defects existing in the prior art, the purpose of the present invention is to provide a non-metallic B-doped β-phase MnO2 electrode material and a preparation method and application thereof, so as to solve or at least partially solve the above-mentioned technical defects existing in the prior art.
[0007] In order to achieve one of the above purposes of the present invention, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing a non-metallic B-doped β-phase MnO2 electrode material, the method specifically comprising the following steps:
[0009] (1) At room temperature, weigh a water-soluble manganese salt and a strong oxidizing compound in a certain proportion and pour them into a beaker, add a certain amount of deionized water, and stir evenly;
[0010] (2) According to the molar ratio of doping, weigh a small amount of boron source and add it to the uniform solution of step (1), and continue to stir evenly;
[0011] (3) pouring the solution prepared in step (2) into a polytetrafluoroethylene liner, and then placing the liner into a stainless steel high-pressure reactor lined with Teflon for hydrothermal reaction;
[0012] (4) After the reaction is completed, the product is filtered, dried and collected.
[0013] Furthermore, in the above technical solution, the water-soluble manganese salt in step (1) includes at least one of manganese sulfate, manganese chloride, manganese nitrate, manganese acetate, etc.
[0014] Furthermore, in the above technical solution, the strong oxidizing compound in step (1) includes at least one of ammonium persulfate, potassium chlorate, concentrated sulfuric acid, etc.
[0015] Furthermore, in the above technical solution, the amount of the water-soluble manganese salt in step (1) is 1 mmol to 1000 mmol, the amount of the strong oxidizing compound is 1 mmol to 1000 mmol, and the amount of deionized water is 5 ml to 5000 ml.
[0016] Furthermore, the above technical solution, as a preferred embodiment of the present invention, the solution in step (1) can be prepared as follows:
[0017] (a) At room temperature, clean a 150 ml beaker and set aside for later use. Then, weigh 20 mmol, or 3.3804 g, of manganese sulfate using weighing paper and pour it into the clean beaker.
[0018] (b) At room temperature, continue to use weighing paper to weigh 20 mmol, i.e. 4.564 g, of ammonium persulfate and gently pour it into the beaker in (a);
[0019] (c) At room temperature, clean a 100 ml graduated cylinder and use it to weigh 100 ml of deionized water. Gently pour the weighed deionized water into the beaker in (b);
[0020] (d) The mixed solution in (c) is placed on a magnetic stirrer and stirred to completely dissolve. The solution after stirring is clear and transparent.
[0021] Furthermore, in the above technical solution, the boron source described in step (2) includes at least one of compounds or organic substances such as boric acid, sodium borate, borax, and diborane.
[0022] Furthermore, in the above technical solution, boric acid is selected as the boron source, the amount of boric acid used is 0.01mmol to 100mmol, and the preferred ratio of the doped boric acid to the water-soluble manganese salt is 1:10, 1:20, or 1:40.
[0023] Furthermore, in the above technical solution, the hydrothermal reaction in step (3) is completed in a drying oven, wherein the temperature of the drying oven is set to 80-300° C., and the reaction time is set to 1-60 hours.
[0024] Furthermore, in the above technical solution, the temperature of the drying oven is set to 180° C., and the reaction time is set to 12 hours.
[0025] Furthermore, in the above technical scheme, the filtration in step (4) is to take out the product of the hydrothermal reaction, pour it into a pre-cleaned suction filtration device, and then wash and filter it several times with deionized water and ethanol or acetone, wherein the filtered powder sample is collected with filter paper, and after cleaning, the collected powder sample is placed in a drying oven to dry.
[0026] Furthermore, the temperature of the drying oven is set at 60° C., and the drying time is at least 8 hours.
[0027] The second object of the present invention is to use the non-metallic B-doped β-phase MnO2 material obtained using the above steps.
[0028] The third object of the present invention is to use the non-metallic B-doped β-phase MnO2 electrode material prepared by the above-mentioned method in aqueous zinc ion batteries.
[0029] A positive electrode material for an aqueous zinc ion battery comprises a non-metallic B-doped β-phase MnO2 electrode material prepared by the method described above.
[0030] Furthermore, in the above technical solution, the aqueous zinc ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte and a battery shell, wherein the positive electrode sheet is composed of a positive electrode active material, a conductive agent and a binder. The non-metallic B-doped β-phase MnO2 electrode material of the present invention is used in the positive electrode active material in the positive electrode sheet of the aqueous zinc ion battery.
[0031] Furthermore, the specific preparation process of the non-metal B-doped β-phase MnO2 electrode material used in the aqueous zinc-ion battery is: use the non-metal B-doped β-phase MnO2 material as the positive electrode active material, acetylene black as the conductive agent, and polytetrafluoroethylene (PTFE) or polyvinylidene fluoride (PVDF) as the adhesive. After the three materials are evenly mixed, N-methylpyrrolidone (NMP) is dropped into them, and the electrode slurry is obtained after even grinding. The prepared electrode slurry is coated on the current collector, put into a drying oven for drying, and then pressed and sliced to obtain the positive electrode sheet of the aqueous zinc-ion battery.
[0032] Furthermore, in the above technical solution, the positive electrode active material, the conductive agent, and the binder are preferably in a mass ratio of 7:2:1, and N-methylpyrrolidone (NMP) is added in an amount that can dilute the mixture to a viscous state.
[0033] Furthermore, in the above technical solution, the electrode slurry is preferably evenly applied on the stainless steel mesh.
[0034] Furthermore, in the above technical solution, the drying temperature of the drying oven is preferably set to 60° C., and the drying time is preferably set to more than 12 hours.
[0035] The reaction mechanism of the present invention is as follows:
[0036] (1) After non-metallic B doped β-phase MnO2, its charge transfer resistance decreased, indicating that non-metallic B doping enhanced the insertion and extraction of Zn ions during the cycle, improved the conductivity, and accelerated the rapid transfer of ions.
[0037] (2) A small amount of non-metallic B ions replace the Mn ions in MnO2, enhancing the redox ability of Mn ions, inhibiting the conversion of Mn ions to divalent soluble Mn ions, improving the cycle stability of the battery, and enhancing the electrochemical performance of the battery.
[0038] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0039] (1) The present invention adopts a one-step hydrothermal method to synthesize a non-metallic B-doped β-phase MnO2 electrode material. The preparation process is simple and can be completed in one step, which greatly simplifies the experimental procedure, saves manpower and material resources, facilitates industrial implementation and application, and has broad market prospects.
[0040] (2) The non-metallic B-doped β-phase MnO2 electrode material of the present invention has high specific capacity and long cycle stability when used in aqueous zinc ion batteries. After 1000 cycles at a current density of 2A / g, the specific capacity drops from 136.2mAh / g to 119.8mAh / g, and the specific capacity retention rate is 87.96%. In the cycle life at a current density of 1A / g, the specific capacity drops from 185.31mAh / g to 156.03mAh / g after 950 cycles, and the specific capacity retention rate is 84.20%. It can be seen from the AC impedance test that B doping can improve the conductivity and accelerate the rapid transfer of ions. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 (a), (b), (c), and (d) correspond to the SEM morphology images of the pure β-phase MnO2 prepared in Example 1 and the non-metallic B-doped β-phase MnO2 electrode materials prepared in Examples 2-4, respectively;
[0042] Figure 2 It is the XRD diffraction pattern of the pure β-phase MnO2 prepared in Example 1 and the non-metallic B-doped β-phase MnO2 electrode material prepared in Examples 2-4;
[0043] Figure 3 It is a comparison chart of the rate performance of batteries prepared using the pure β-phase MnO2 of Example 1 and the non-metallic B-doped β-phase MnO2 electrode materials of Examples 2-4;
[0044] Figure 4 is a comparison chart of the cycle life of the batteries obtained in Example 1 and Example 3 at a current density of 1 A / g;
[0045] Figure 5 is a graph of cyclic voltammetry (CV) test results of the battery obtained in Example 3;
[0046] Figure 6 is an electrochemical impedance spectroscopy (EIS) test result diagram of the battery obtained in Examples 1 to 4;
[0047] Figure 7 is a CP diagram of the specific capacity of the battery obtained in Example 3 at different current densities;
[0048] Figure 8 It is a comparison chart of the cycle life of the batteries obtained in Examples 1 to 4 at a current density of 2 A / g. DETAILED DESCRIPTION
[0049] The present invention is further described in detail below through implementation cases. A creative detailed operation process is given according to the content of the present invention, but the protection scope of the present invention is not limited to the following implementation cases, because technical experts in this field or related fields can easily make various forms of changes to the precise description of the present invention, but in fact do not deviate from the spirit and scope of the claims attached to the present invention, so no matter what changes are made to the embodiments of the present invention by technical experts in this field or related fields, they are all covered within the scope of the attached claims. In fact, the specific numerical values used in this application, including numbers, percentages, and other sample dosage instructions, should be understood as "approximately" modified, and each numerical value should be understood as obtained based on significant figures or rounded off.
[0050] The following specific implementation cases are all experimental processes based on the packaging test of button batteries, which include a positive electrode (non-metal B doped β-phase MnO2 electrode material), a hydrophilic fiber separator, a commercial zinc sheet negative electrode, a neutral electrolyte (2MZnSO4+0.2M MnSO4) and a button battery shell. In the implementation cases of the present invention, unless otherwise specified, the experimental methods are conventional methods, and the raw materials and reagents can be obtained from conventional commercial sources such as commercial purchases.
[0051] Example 1
[0052] The method for preparing a pure β-phase MnO2 electrode material of this embodiment includes the following steps:
[0053] (1) Solution configuration:
[0054] (a) At room temperature, clean a 150 ml beaker and set aside for later use. Then, weigh 20 mmol, or 3.3804 g, of manganese sulfate using weighing paper and pour it into the clean beaker.
[0055] (b) At room temperature, continue to use weighing paper to weigh 20mmol, or 4.564g, of ammonium persulfate and gently pour it into the beaker in (a);
[0056] (c) At room temperature, clean a 100 ml graduated cylinder and use it to weigh 100 ml of deionized water. Gently pour the weighed deionized water into the beaker in (b);
[0057] (d) The mixed solution in (c) is placed on a magnetic stirrer and stirred to completely dissolve. The solution after stirring is clear and transparent.
[0058] (2) Hydrothermal reaction:
[0059] The final mixed solution prepared in the above step (1) was poured into a polytetrafluoroethylene liner, and then the liner was placed in a stainless steel high-pressure reactor lined with Teflon. After the reactor was tightened, it was placed in a drying oven for hydrothermal reaction. At this time, the reaction temperature of the drying oven was set to 180°C and the reaction time was 12 hours.
[0060] (3) Filtration:
[0061] Clean the filtration device in advance and set it aside. After the hydrothermal reaction of the solution in the drying box is completed and the temperature in the box reaches room temperature, open the drying box, take out the stainless steel high-pressure reactor, unscrew it and take out the polytetrafluoroethylene liner at room temperature, collect the product in the solution with filter paper, and rinse it repeatedly with deionized water at least 2 times, and then rinse it with anhydrous ethanol at least 2 times.
[0062] (4) Drying:
[0063] After cleaning, collect the clean β-phase MnO2 powder sample after filtration and put it into a drying oven for drying. The drying temperature is set to 60°C and the drying time is at least 8 hours. After drying, collect the powder sample and mark it. This powder sample is the pure β-phase MnO2 electrode material.
[0064] Preparation of electrodes:
[0065] The collected pure β-phase MnO2 powder sample is used as the positive electrode active material, acetylene black is used as the conductive agent, and polytetrafluoroethylene (PTFE) is used as the adhesive. The three materials are weighed by weighing paper to 70 mg, 20 mg, and 10 mg respectively. After weighing, they are put into a grinding dish and mixed and ground evenly. Then 1 ml of N-methylpyrrolidone (NMP) is dropped and ground evenly again to obtain a viscous electrode slurry. The obtained electrode slurry is coated on a stainless steel mesh current collector cut in advance with a size of 3 cm×6 cm. After the smearing is evenly applied, the mass of active material per square centimeter is made to be about 1.5 mg. Then, it is put into a drying oven set at a temperature of 60°C and dried for 12 hours, and then taken out for tableting and slicing to obtain the aqueous zinc ion battery positive electrode sheet made by the present invention.
[0066] Battery assembly: first place the positive electrode sheet in the center of the positive electrode shell, soak the hydrophilic diaphragm with 2M ZnSO4+0.2MMnSO4 composite neutral salt aqueous electrolyte and then stack it on the positive electrode sheet, place the commercial zinc sheet on the other side of the hydrophilic diaphragm so that it is opposite to the positive electrode sheet, and finally add the gasket, spring and negative electrode shell in sequence, place the assembled battery on the battery packaging machine for packaging, and after packaging is completed, the battery can be removed for use.
[0067] Electrochemical performance test: The battery obtained in this embodiment is tested for rate performance and cycle life using a new eight-channel battery testing device (NEWARE). Both rate performance and cycle life are charged and discharged using constant current. The voltages are set to a charging voltage of 1.85 V and a discharge voltage of 1 V. The current densities of the rate performance are set to 0.1 A / g, 0.2 A / g, 0.3 A / g, 0.5 A / g, 0.8 A / g, 1.0 A / g, 2.0 A / g, 5.0 A / g, 7.0 A / g, and 10 A / g, respectively. It can be seen from the test results that after cycle tests at different current densities, the battery can still operate at the same current density with the same high specific capacity. The test cycle life current density is set to 2 A / g. From the test results, it can be seen that the initial specific capacity of pure β-phase MnO2 is 93.39 mAh / g, and the specific capacity is still 39.44 mAh / g after 1000 cycles. The battery obtained in Example 1 was subjected to cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS) tests using a Chenhua electrochemical workstation (CHI760E). The initial and final voltages of the cyclic voltammetry test were set to 1 V, the maximum voltage was set to 1.85 V, the voltage scan rate was 1 mV / s, and the EIS test frequency was set to 10 -2 Hz-10 6 Hz, the voltage is set to open circuit voltage.
[0068] Example 2
[0069] The method for preparing a non-metallic B-doped β-phase MnO2 electrode material of this embodiment includes the following steps:
[0070] (1) Solution configuration:
[0071] (a) At room temperature, clean a 150 ml beaker and set aside for later use. Then, weigh 20 mmol, or 3.3804 g, of manganese sulfate using weighing paper and pour it into the clean beaker.
[0072] (b) At room temperature, continue to use weighing paper to weigh 20mmol, or 4.564g, of ammonium persulfate and gently pour it into the beaker in (a);
[0073] (c) At room temperature, clean a 100 ml graduated cylinder and use it to weigh 100 ml of deionized water. Gently pour the weighed deionized water into the beaker in (b);
[0074] (d) The mixed solution in (c) is placed on a magnetic stirrer and stirred to completely dissolve. The solution after stirring is clear and transparent.
[0075] (e) At room temperature, 2 mmol, or 0.12366 g, of boric acid is weighed with weighing paper and poured into the evenly stirred solution in (d), and the solution is continued to be stirred on a magnetic stirrer to completely dissolve the boron. The ratio of boron to manganese doping is 1:10.
[0076] (2) Hydrothermal reaction:
[0077] The final mixed solution prepared in the above step (1) was poured into a polytetrafluoroethylene liner, and then the liner was placed in a stainless steel high-pressure reactor lined with Teflon. After the reactor was tightened, it was placed in a drying oven for hydrothermal reaction. At this time, the reaction temperature of the drying oven was set to 180°C and the reaction time was 12 hours.
[0078] (3) Filtration:
[0079] Clean the filtration device in advance and set it aside. After the hydrothermal reaction of the solution in the drying box is completed and the temperature in the box reaches room temperature, open the drying box, take out the stainless steel high-pressure reactor, unscrew it and take out the polytetrafluoroethylene liner at room temperature, collect the product in the solution with filter paper, and rinse it repeatedly with deionized water at least 2 times, and then rinse it with anhydrous ethanol at least 2 times.
[0080] (4) Drying:
[0081] After cleaning, the non-metallic B-doped β-phase MnO2 powder sample that has been cleaned by filtration is collected and placed in a drying oven for drying. The drying temperature is set to 60°C and the drying time is at least 8 hours. After drying, the powder sample is collected and marked. This powder sample is non-metallic B-doped β-phase MnO2.
[0082] Preparation of electrodes:
[0083] The collected non-metallic B-doped β-phase MnO2 powder sample is used as the positive electrode active material, acetylene black is used as the conductive agent, and polytetrafluoroethylene (PTFE) is used as the adhesive. The three materials are weighed by weighing paper to 70 mg, 20 mg, and 10 mg respectively. After weighing, they are put into a grinding dish and mixed and ground evenly. Then 1 ml of N-methylpyrrolidone (NMP) is dropped and ground evenly again to obtain a viscous electrode slurry. The obtained electrode slurry is coated on a stainless steel mesh current collector cut in advance with a size of 3 cm×6 cm. After the smearing is evenly applied, the mass of the active substance per square centimeter is as much as possible to be about 1.5 mg. Then, it is put into a drying oven set at a temperature of 60°C and dried for 12 hours, and then taken out for tableting and slicing to obtain the aqueous zinc ion battery positive electrode sheet made by the present invention.
[0084] Battery assembly: first place the positive electrode sheet in the center of the positive electrode shell, soak the hydrophilic diaphragm with 2M ZnSO4+0.2MMnSO4 composite neutral salt aqueous electrolyte and then stack it on the positive electrode sheet, place the commercial zinc sheet on the other side of the hydrophilic diaphragm so that it is opposite to the positive electrode sheet, and finally add the gasket, spring and negative electrode shell in sequence, place the assembled battery on the battery packaging machine for packaging, and after packaging is completed, the battery can be removed for use.
[0085] Electrochemical performance test: The battery obtained in this embodiment is tested for rate performance and cycle life using a new eight-channel battery test device (NEWARE). Both rate performance and cycle life are charged and discharged using constant current, and the voltages are set to a charging voltage of 1.85 V and a discharge voltage of 1 V. The current densities of the rate performance are set to 0.1 A / g, 0.2 A / g, 0.3 A / g, 0.5 A / g, 0.8 A / g, 1.0 A / g, 2.0 A / g, 5.0 A / g, 7.0 A / g, and 10 A / g, respectively. The test results show that after cycle tests at different current densities, the battery can still operate at the same current density with the same high specific capacity. The test cycle life current density is set to 2 A / g. From the test results, it can be seen that the initial specific capacity of non-metallic B doped β-phase MnO2 (doping ratio of 1:10) is 167.93 mAh / g, and the specific capacity is still 81.12 mAh / g after 1000 cycles. The battery obtained in Example 1 was subjected to cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS) tests using a Chenhua electrochemical workstation (CHI760E). The initial and final voltages of the cyclic voltammetry test were set to 1 V, the maximum voltage was set to 1.85 V, the voltage scan rate was 1 mV / s, and the EIS test frequency was set to 10 -2 Hz-10 6 Hz, the voltage is set to open circuit voltage.
[0086] Example 3
[0087] The preparation method of a non-metallic B-doped β-phase MnO2 electrode material in this embodiment is basically the same as that in Example 2, except that the B doping ratio during solution configuration is changed. At room temperature, 1 mmol, i.e., 0.06183 g of boric acid is weighed with weighing paper and poured into a mixed solution of manganese sulfate and ammonium persulfate and stirred evenly to dissolve it completely, wherein the B-doped Mn ratio is 1:20. Other processes are the same, including the preparation of electrodes, battery assembly, and electrochemical performance testing processes. Due to the different doping ratios, the test results have also changed. The powder sample of non-metallic B-doped β-phase MnO2 (doping ratio of 1:20) prepared in this embodiment is used to make electrode materials for use in aqueous zinc ion batteries. The specific capacity at different current densities in its rate performance is improved compared with that in Example 2. When the cycle current density is set to 2A / g, the initial specific capacity drops from 136.2 mAh / g to 119.8 mAh / g, and the specific capacity retention rate is 87.96%.
[0088] Example 4
[0089] The preparation method of a non-metallic B-doped β-phase MnO2 electrode material in this embodiment is basically the same as that in Example 2, except that the B doping ratio during solution configuration is changed. At room temperature, 0.5mmol, i.e., 0.030915g of boric acid is weighed with weighing paper and poured into a mixed solution of manganese sulfate and ammonium persulfate, and stirred evenly to dissolve it completely, wherein the B-doped Mn ratio is 1:40. Other processes are the same, including the preparation of electrodes, battery assembly, and electrochemical performance testing processes. Due to the different doping ratios, the test results have also changed. The powder sample of non-metallic B-doped β-phase MnO2 (doping ratio of 1:40) prepared in this embodiment is used to make electrode materials for use in aqueous zinc ion batteries. The specific capacity at different current densities in its rate performance is slightly lower than that in Example 2. When the cycle current density is set to 2A / g, the initial specific capacity drops from 164.12mAh / g to 75.45mAh / g.
[0090] Figure 1 A JSM-7100F scanning electron microscope (SEM) produced by JEOL of Japan was used to observe the morphology and structure of the samples. Figure 1(a), (b), (c), and (d) correspond to the microscopic morphologies of the pure β-phase MnO2 prepared in Example 1 and the non-metallic B-doped β-phase MnO2 electrode material samples prepared in Examples 2-4, respectively. It can be seen that the morphologies of the four SEM images are all rod-like structures with a thickness of about 0.05um to 0.25um and a length of about 0.5um to 2.5um. The morphologies of the β-phase MnO2 doped with non-metallic B in Figures (b), (c), and (d) are more regular than the undoped pure β-phase MnO2 rod-like structure in Figure (a), and the two ends of the rods are smoother.
[0091] Figure 2 The XRD diffraction pattern was obtained using a Bruker D8 Advance X-ray diffractometer under CuKα radiation of 40 kV and 40 mA. The corresponding figure of Example 1 shows pure β-phase MnO2, the corresponding figure of Example 2 shows a B-doped Mn ratio of 1:10, the corresponding figure of Example 3 shows a B-doped Mn ratio of 1:20, and the corresponding figure of Example 4 shows a B-doped Mn ratio of 1:40. It can be seen that the XRD diffraction patterns of both pure β-phase MnO2 and B-doped β-phase MnO2 can correspond to the standard card PDF#24-0735, indicating that a small amount of B doping does not change the structure of β-phase MnO2.
[0092] Figure 3 The batteries obtained in Examples 1 to 4 were tested for rate performance using NEWARE eight-channel battery testing equipment. The specific capacities of B-doped β-phase MnO2 in Examples 2 to 4 were higher than that of pure β-phase MnO2 in Example 1, and the specific capacities could reach 451.12 mAh / g at a low current density of 0.1 A / g.
[0093] Figure 4 The batteries obtained in Example 1 and Example 3 were tested for cycle life at a current density of 1 A / g using a new eight-channel battery tester (NEWARE). By comparing the rate performance of Examples 1 to 4 and the cycle life at a current density of 2 A / g, it can be seen that the capacity and stability of the β-phase MnO2 with a B-doped Mn ratio of 1:20 in Example 3 are the best, so Figure 4 The cycle life of the β-phase MnO2 with a B-doped Mn ratio of 1:20 in Example 3 and the pure β-phase MnO2 in Example 1 at a current density of 1A / g shows that the specific capacity of the β-phase MnO2 with a B-doped Mn ratio of 1:20 drops from 185.31mAh / g to 156.03mAh / g after 950 cycles, and the specific capacity retention rate is 84.20%. The specific capacity of the pure β-phase MnO2 drops from 160.27mAh / g to 36.50mAh / g after 950 cycles, and the specific capacity retention rate is only 22.78%.
[0094] Figure 5The battery obtained in Example 3 was subjected to cyclic voltammetry (CV) test using a Chenhua electrochemical workstation (CHI760E), with a voltage sweep rate of 1 mV / s and a voltage setting range of 1 to 1.85 V. It can be seen from the figure that the reversibility repeatability of the first and third cycles is relatively strong.
[0095] Figure 6 The batteries obtained in Examples 1 to 4 were subjected to electrochemical impedance spectroscopy (EIS) testing using a Chenhua electrochemical workstation (CHI760E). The test frequency was set to 10 -2 Hz-10 6 Hz, the voltage is set to the open circuit voltage. It can be seen from the AC impedance fitting diagram that the internal resistance of the battery internal materials of Examples 1 to 4 does not change much, but the charge transfer resistance becomes smaller after B doping, among which the charge transfer resistance in Example 3 is the smallest, indicating that B doping can improve the conductivity and accelerate the rapid transfer of ions.
[0096] Figure 7 The battery obtained in Example 3 uses the new eight-channel battery test equipment (NEWARE) to test the specific capacity CP diagram of the battery at different current densities. It can be clearly seen that the specific capacity changes from 5A / g to 0.1A / g. As the current density decreases, the specific capacity gradually increases, from 5A / g specific capacity 76.6mAh / g to 0.1A / g specific capacity 389.3mAh / g. Through the CP diagram of small current, we can see two discharge platforms, and the discharge platform that contributes more to the specific capacity is the embedding process of Zn ions.
[0097] Figure 8 The battery obtained in Examples 1 to 4 is tested by the new eight-channel battery test equipment (NEWARE) at a current density of 2A / g. The data comparison shows that the capacity and stability of the β-phase MnO2 with a B-doped Mn ratio of 1:20 in Example 3 are the best, wherein the B-doped 1:20 has a specific capacity of 136.2mAh / g at a current density of 2A / g and a specific capacity retention rate of 87.96%, while the specific capacity of the pure β-phase MnO2 has a specific capacity of 97.3mAh / g at a current density of 2A / g and a specific capacity retention rate of only 40.49%. It can be seen that the capacity and stability of the β-phase MnO2 are enhanced by B doping.
Claims
1. Application of a non-metallic B-doped β-phase MnO2 electrode material in an aqueous zinc ion battery, the aqueous zinc ion battery comprising a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte and a battery shell; the positive electrode sheet is composed of a positive electrode active material, a conductive agent, and a binder; characterized in that: The positive electrode active material is a non-metallic B-doped β-phase MnO2 electrode material, and the non-metallic B-doped β-phase MnO2 electrode material has a rod-shaped structure; the non-metallic B-doped β-phase MnO2 electrode material is prepared by the following method, and the specific steps are as follows: (1) At room temperature, weigh a water-soluble manganese salt and a strong oxidizing compound in a certain proportion and pour them into a beaker, add a certain amount of deionized water, and stir evenly; the specific steps are as follows: (a) At room temperature, clean a 150 ml beaker and set aside. Then weigh 20 mmol of manganese sulfate using weighing paper and pour it into the clean beaker. (b) At room temperature, continue to use weighing paper to weigh 20mmol of ammonium persulfate and gently pour it into the beaker in (a); (c) At room temperature, clean a 100 ml graduated cylinder and use it to weigh 100 ml of deionized water. Gently pour the weighed deionized water into the beaker in (b); (d) The mixed solution in (c) is placed on a magnetic stirrer and stirred to completely dissolve, and the solution after stirring is clear and transparent; (2) According to the molar ratio of doping, weigh a small amount of boric acid and add it to the uniform solution in (1), and continue to stir evenly; the ratio of doped boric acid to water-soluble manganese salt is 1:20; (3) Pour the prepared solution into a polytetrafluoroethylene liner, and then place the liner into a stainless steel high-pressure reactor lined with Teflon for hydrothermal reaction; the hydrothermal reaction is completed in a drying oven, the temperature of the drying oven is set to 180°C, and the reaction time is set to 12 hours; (4) After the reaction is completed, the product is filtered, dried and collected.
2. The use according to claim 1, characterized in that: The mass ratio of the positive electrode active material, the conductive agent, and the binder is 7:2:1.