Glass etching liquid, method for producing lithium aluminum silicon glass surface with starlight effect, and mobile phone case

By using a swing etching process of using acidic mixed solutions and ammonium fluoride and other raw materials on the surface of lithium aluminum silicon glass, a micron-scale crystal diamond particle structure is formed, which solves the problems of easy aging and poor adhesion of decorative glass in the prior art, and realizes lithium Aluminum-silicon glass material has star-bright effect and excellent durability.

CN116217085BActive Publication Date: 2024-11-05XUCHANG HENGHAO OPTICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211557688.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-11-05
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

When existing decorative glass products achieve star-bright effects, the physical spraying process has problems such as aging, scratching, poor adhesion and short life cycle.

Method used

A mixed solution of highly acidic sulfuric acid and nitric acid is used as a carrier, and a glass etching solution is prepared by combining ammonium fluoride, ammonium fluoride borate, copper sulfate, ammonium nitrate, polyethylene glycol and gum. The glass etching solution is prepared by swinging etching process on the surface of lithium aluminum silicon glass Form an irregular and loose micro-scale crystal diamond particle structure to achieve a star-stunning effect.

Benefits of technology

The generated lithium-aluminum silicon glass surface has good anti-glare, scratch resistance, dust resistance and fingerprint resistance, while extending the product life cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116217085B_ABST
    Figure CN116217085B_ABST
Patent Text Reader

Abstract

The invention discloses a glass etching liquid and a method for making a starlight effect on the surface of lithium aluminum silicate glass and a mobile phone shell. The glass etching liquid is composed of sulfuric acid, nitric acid, ammonium fluoride, ammonium fluoroborate, copper sulfate, ammonium nitrate, polyethylene glycol, gum and water. The invention selects a mixed solution of sulfuric acid and nitric acid with strong acidity as a carrier to provide abundant hydrogen ions, adds ammonium fluoride and ammonium fluoroborate as main etching raw materials, and simultaneously adds a certain proportion of surfactant and viscosity regulator to prepare the glass etching liquid. The aging etching liquid can form a micron-level irregularly loosely arranged crystal diamond particle structure layer on the surface of lithium aluminum silicate glass under the condition of swing etching process. When facing the light, the glass surface presents a bright and shining effect like stars in the night sky, and the etched glass has good anti-glare, anti-scratch, anti-dust, anti-fingerprint and other excellent properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glass chemical etching, and specifically relates to a glass etching liquid and a manufacturing method for making a lithium aluminum silicon glass mobile phone back shell have a starlight effect by using the glass etching liquid. Background Art

[0002] With the saturation of the smart phone market, people's demand for personalization and novelty of mobile phones is also increasing day by day. More and more mobile phone manufacturers rely on novel appearance decoration effects to attract consumers. The present invention is based on satisfying consumers' curiosity and launches a mobile phone back shell product with a starry effect. Under the illumination of light, the back shell of the mobile phone presents a starry effect, as bright and dazzling as the stars in the night sky, giving consumers a pleasing visual experience. At present, in the field of decorative glass production, to achieve the starry effect on the glass surface, a process combining spraying resin and metal glitter powder is generally used. The products produced by this physical spraying process have defects such as easy aging, easy scratching, poor adhesion, and short life cycle. Summary of the invention

[0003] In view of the defects of the physical spraying process in the prior art, the present invention provides a chemical acid etching technology, which performs acid etching on the back shell of lithium aluminum silicon glass material to form irregularly loosely arranged micro crystal diamond particles on the glass surface, thereby producing a starry visual effect on the glass surface.

[0004] The object of the present invention is achieved in the following manner:

[0005] A glass etching solution comprises the following raw materials in mass percentage (wt%): 12-20% sulfuric acid, 15-25% nitric acid, 20-30% ammonium fluoride, 5-15% ammonium fluoroborate, 2-8% copper sulfate, 3-10% ammonium nitrate, 0.3-1.5% polyethylene glycol, 1-3% gum and 20-35% water.

[0006] The method for producing a star-lit effect on the surface of lithium aluminum silicate glass comprises the following steps:

[0007] a. Mix the raw materials in the above glass etching solution ratio and stir well to obtain a uniform and stable supersaturated solution state, and allow to stand and mature at room temperature;

[0008] b. The side of the lithium aluminum silicate glass sheet that does not need to be etched is protected by silk screen coating with anti-etching ink.

[0009] c. Clean the side of the lithium aluminum silicate glass substrate to be etched with pure water, and place it in the etching solution for swing etching in a wet state;

[0010] d. Take out the etched lithium aluminum silicate glass original sheet from the etching solution, clean it with pure water and air dry it.

[0011] In step a, the mixture is left to stand and mature for 72 hours.

[0012] In step c, the swing etching controls the swing stroke to be 300-500 mm and the swing frequency to be 60-80 times / minute.

[0013] In step c, the temperature of the etching solution is controlled to be 10-15°C.

[0014] In step c, the swing etching time is controlled to be 3-5 minutes.

[0015] A mobile phone case is prepared by the above-mentioned manufacturing method, and the mobile phone back case made of lithium aluminum silicate glass has a star-lit effect.

[0016] Compared with the prior art, the present invention selects a mixed solution of highly acidic sulfuric acid and nitric acid as a carrier to provide abundant hydrogen ions, adds ammonium fluoride and ammonium fluoroborate as main etching raw materials, and simultaneously adds a certain proportion of surfactant and viscosity regulator to prepare a glass etching solution. The matured etching solution can form a micron-scale irregularly loosely arranged crystal diamond particle structure layer on the surface of lithium aluminum silicon glass under the conditions of the swing etching process (see electron microscope image). When facing the light, the glass surface presents a bright and shining effect like stars in the night sky. The etched glass has excellent properties such as good anti-glare, anti-scratch, anti-dust, and anti-fingerprint. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a 64x electron microscope image of the surface of lithium aluminum silicate glass after etching.

[0018] Figure 2 It is a schematic diagram of the lithium aluminum silicon glass mobile phone back shell after etching of the present invention. DETAILED DESCRIPTION

[0019] The present invention is further described below in conjunction with specific embodiments and drawings, but the present invention is not limited thereto.

[0020] A glass etching solution comprises the following raw materials in mass percentage (wt%): 12-20% sulfuric acid, 15-25% nitric acid, 20-30% ammonium fluoride, 5-15% ammonium fluoroborate, 2-8% copper sulfate, 3-10% ammonium nitrate, 0.3-1.5% polyethylene glycol, 1-3% gum and 20-35% water.

[0021] The method for producing a star-lit effect on the surface of lithium aluminum silicate glass comprises the following steps:

[0022] a. Mix the raw materials in the above glass etching solution in the proportions described above, and stir well to give a uniform and stable supersaturated solution state, and allow to stand at room temperature for 72 hours;

[0023] b. The side of the lithium aluminum silicate glass sheet that does not need to be etched is protected by silk screen coating with anti-etching ink.

[0024] c. Clean the side of the lithium aluminum silicate glass substrate to be etched with pure water, put it into the etching solution in a wet state for swing etching, control the swing stroke of the swing etching to 300-500mm, the swing frequency to 60-80 times / minute, control the etching solution temperature to 10-15°C, and the swing etching time to 3-5 minutes;

[0025] d. Take out the etched lithium aluminum silicate glass original sheet from the etching solution, clean it with pure water and air dry it.

[0026] According to the composition and characteristics of lithium aluminosilicate glass, sulfuric acid, nitric acid, ammonium fluoride, ammonium fluoroborate, copper sulfate, ammonium nitrate, polyethylene glycol, gum, and water are selected to prepare the etching solution. The functions of various raw materials in the etching solution are as follows:

[0027] Sulfuric acid and nitric acid: provide hydrogen ions to replace the metal cations in the lithium aluminum silicate glass to form a silicate gel layer, providing the basic conditions for fluoride ions to corrode the skeleton in the glass.

[0028] Ammonium fluoride and ammonium fluoroborate: They provide fluoride ions in acidic solutions to corrode the silica skeleton and alumina skeleton in the glass to form a fluorosilicate etching particle layer, which plays a major etching role.

[0029] Copper sulfate and ammonium nitrate: provide metal ions or ammonium ions to coordinate and replace the lattice of the attachment layer. With the help of the lattice coordination and replacement of cations, crystal particles of certain specifications and shapes are formed. These crystal particles grow in a certain direction, thereby generating a micron-sized crystal diamond particle structure on the glass surface (see electron microscope image).

[0030] Polyethylene glycol: Introduced as a surfactant, it can effectively increase the wettability between the solution and the glass surface, maintain the uniformity and consistency of the etching reaction, and reduce etching defects.

[0031] Gum: Introduced as a viscosity modifier, it can increase the suspension effect of the etching solution, making the etching effect more lasting and uniform.

[0032] The present invention adopts a chemical acid etching process to produce a star-studded modification effect on the surface of lithium aluminum silicate glass, selects a mixed solution of sulfuric acid and nitric acid with strong acidity as a carrier, provides abundant hydrogen ions, adds ammonium fluoride and ammonium fluoroborate as main etching raw materials, and simultaneously adds a certain proportion of surfactant and viscosity regulator to prepare a glass etching liquid. The matured etching liquid can form a micron-level irregularly loosely arranged crystal diamond particle structure layer on the surface of the lithium aluminum silicate glass under the condition of a swing etching process (see an electron microscope image). In the case of facing the light, the glass surface presents a bright and shining effect like stars in the night sky, and the etched glass has excellent properties such as good anti-glare, anti-scratch, anti-dust, and anti-fingerprint.

[0033] A mobile phone case is prepared according to the above-mentioned manufacturing method, and the mobile phone back case made of lithium aluminum silicate glass has a star-studded effect.

[0034] Example 1

[0035] The glass etching solution has the following raw materials in mass percentage (Wt%): 12.5% ​​sulfuric acid, 22.5% nitric acid, 25% ammonium fluoride, 8.5% ammonium fluoroborate, 5% copper sulfate, 3.5% ammonium nitrate, 0.3% polyethylene glycol, 1.2% gum, and 21.5% water.

[0036] The manufacturing method of lithium aluminum silicon glass mobile phone back cover with starlight effect comprises the following specific steps:

[0037] a. Prepare glass etching solution. According to the etching process requirements, add the above-mentioned raw materials in the mass percentage into water in turn, stir well to make the solution present a uniform and stable supersaturated solution state, and let it stand and mature for 72 hours at room temperature.

[0038] b. The side of the lithium aluminum silicate glass sheet that does not need to be etched is protected by silk-screen coating with anti-etching ink.

[0039] c. Clean the side of the lithium aluminum silicate glass substrate that needs to be etched with pure water, and put it into the etching solution in a wet state for swing etching. Control the swing stroke to 300mm, the swing frequency to 80 times / minute; control the etching solution temperature to 12℃, and the swing etching time to 3.5 minutes.

[0040] d. Take out the lithium aluminum silicon glass original sheet that has reached the etching time requirement and completed the etching process from the etching solution in time, clean it with pure water and air dry it.

[0041] The photo with starlight effect is obtained by etching lithium aluminum silicate glass with the etching solution configured in this embodiment. Figure 1 According to the manufacturing method of this embodiment, a mobile phone shell is prepared, and the rear shell of the mobile phone made of lithium aluminum silicate glass has a starlight effect, such as Figure 2 shown.

[0042] Example 2

[0043] The glass etching solution has the following raw materials in mass percentage (Wt%): 15.5% sulfuric acid, 18.5% nitric acid, 22.5% ammonium fluoride, 10% ammonium fluoroborate, 3.5% copper sulfate, 5% ammonium nitrate, 0.4% polyethylene glycol, 1.5% gum, and 23.1% water.

[0044] The manufacturing method of lithium aluminum silicon glass mobile phone back cover with starlight effect comprises the following specific steps:

[0045] a. Prepare glass etching solution. According to the etching process requirements, add the above-mentioned raw materials in the mass percentage into water in turn, stir well to make the solution present a uniform and stable supersaturated solution state, and let it stand and mature for 72 hours at room temperature.

[0046] b. The side of the lithium aluminum silicate glass sheet that does not need to be etched is protected by silk-screen coating with anti-etching ink.

[0047] c. Clean the side of the lithium aluminum silicate glass substrate that needs to be etched with pure water, and put it into the etching solution in a wet state for swing etching. Control the swing stroke to 350mm and the swing frequency to 70 times / minute; control the etching solution temperature to 10℃ and the swing etching time to 5 minutes.

[0048] d. Take out the lithium aluminum silicon glass original sheet that has reached the etching time requirement and completed the etching process from the etching solution in time, clean it with pure water and air dry it.

[0049] Example 3

[0050] The glass etching solution has the following raw materials in mass percentage (Wt%): 17.5% sulfuric acid, 15.5% nitric acid, 20.5% ammonium fluoride, 12% ammonium fluoroborate, 3% copper sulfate, 5% ammonium nitrate, 0.3% polyethylene glycol, 1.0% gum, and 25.2% water.

[0051] The manufacturing method of lithium aluminum silicon glass mobile phone back cover with starlight effect comprises the following specific steps:

[0052] a. Prepare glass etching solution. According to the etching process requirements, add the above-mentioned raw materials in the mass percentage into water in turn, stir well to make the solution present a uniform and stable supersaturated solution state, and let it stand and mature for 72 hours at room temperature.

[0053] b. The side of the lithium aluminum silicate glass sheet that does not need to be etched is protected by silk-screen coating with anti-etching ink.

[0054] c. Clean the side of the lithium aluminum silicate glass substrate that needs to be etched with pure water, and put it into the etching solution in a wet state for swing etching. Control the swing stroke to 500mm and the swing frequency to 60 times / minute; control the etching solution temperature to 15℃ and the swing etching time to 3 minutes.

[0055] d. Take out the lithium aluminum silicon glass original sheet that has reached the etching time requirement and completed the etching process from the etching solution in time, clean it with pure water and air dry it.

[0056] According to the unified testing method of the glass industry, the various properties of lithium aluminum silicate glass before and after etching were measured. The specific performance index comparison results are shown in Table 1:

[0057] Table 1

[0058]

[0059] Example 4

[0060] The glass etching solution has the following raw materials in mass percentage (Wt%): 12.0% sulfuric acid, 25.0% nitric acid, 20.0% ammonium fluoride, 6.7% ammonium fluoroborate, 2.0% copper sulfate, 10.0% ammonium nitrate, 1.3% polyethylene glycol, 3.0% gum, and 20% water.

[0061] The method for manufacturing the lithium aluminum silicon glass mobile phone back cover with starlight effect is the same as that in Example 1.

[0062] Example 5

[0063] The glass etching solution has the following raw materials in mass percentage (Wt%): 20.0% sulfuric acid, 15.0% nitric acid, 20.0% ammonium fluoride, 15% ammonium fluoroborate, 4.0% copper sulfate, 3.0% ammonium nitrate, 1.5% polyethylene glycol, 2.0% gum, and 21.5% water.

[0064] The method for manufacturing the lithium aluminum silicon glass mobile phone back cover with starlight effect is the same as that in Example 1.

[0065] Example 6

[0066] The glass etching solution has the following raw materials in mass percentage (Wt%): 13.0% sulfuric acid, 20.0% nitric acid, 21.0% ammonium fluoride, 5% ammonium fluoroborate, 6.2% copper sulfate, 7.3% ammonium nitrate, 1.5% polyethylene glycol, 1.1% gum, and 24.9% water.

[0067] The method for manufacturing the lithium aluminum silicon glass mobile phone back cover with starlight effect is the same as that in Example 1.

[0068] Example 7

[0069] The glass etching solution has the following raw materials in mass percentage (Wt%): 14.0% sulfuric acid, 12.0% nitric acid, 30.0% ammonium fluoride, 5.1% ammonium fluoroborate, 8% copper sulfate, 3.0% ammonium nitrate, 1.0% polyethylene glycol, 2.2% gum, and 24.7% water.

[0070] The method for manufacturing the lithium aluminum silicon glass mobile phone back cover with starlight effect is the same as that in Example 1.

[0071] The above is only a preferred embodiment of the present invention. It should be pointed out that for those skilled in the art, several changes and improvements can be made without departing from the overall concept of the present invention, which should also be regarded as the scope of protection of the present invention.

Claims

1. A method for producing a star-lit effect on the surface of lithium aluminum silicate glass, characterized in that: The following steps are included: a. Mix the raw materials according to 12-20% sulfuric acid, 15-25% nitric acid, 20-30% ammonium fluoride, 5-15% ammonium fluoroborate, 2-8% copper sulfate, 3-10% ammonium nitrate, 0.3-1.5% polyethylene glycol, 1-3% gum, and 20-35% water by mass, and stir well to obtain a uniform and stable supersaturated solution state, and allow to stand and mature at room temperature; b. The side of the lithium aluminum silicate glass sheet that does not need to be etched is protected by silk screen coating with anti-etching ink. c. Clean the side of the lithium aluminum silicate glass substrate to be etched with pure water, and place it in the etching solution for swing etching in a wet state; d. Take out the etched lithium aluminum silicate glass original sheet from the etching solution, clean it with pure water and air dry it.

2. The method for producing the starry effect on the surface of lithium aluminosilicate glass according to claim 1, characterized in that: In step a, the mixture is left to stand and mature for 72 hours.

3. The method for producing the starry effect on the surface of lithium aluminosilicate glass according to claim 1, characterized in that: In step c, the swing etching controls the swing stroke to be 300-500 mm and the swing frequency to be 60-80 times / minute.

4. The method for producing the starlight effect on the surface of lithium aluminosilicate glass according to claim 1, characterized in that: In step c, the temperature of the etching solution is controlled to be 10-15°C.

5. The method for producing the starry effect on the surface of lithium aluminosilicate glass according to claim 1, characterized in that: In step c, the swing etching time is controlled to be 3-5 minutes.

6. A mobile phone rear cover, characterized in that: The mobile phone back cover made of lithium aluminum silicate glass prepared by the manufacturing method according to any one of claims 1 to 5 has a star-studded effect.