Method for producing olefin resin porous body, method for producing battery separator and apparatus for producing battery separator
By mixing olefin resin and solvent in a pressure vessel, and adjusting the phase separation method using the temperature and solubility parameters of high-pressure carbon dioxide, the problem of difficult to control the pore structure in the prior art is solved, and the detailed control of porous bodies and batteries are realized Improved performance of partitions.
Patent Information
- Application Number
- CN202211533763.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-03
- Filing Date
- 2022-12-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-01
AI Technical Summary
The prior art is difficult to effectively control the porous structure of the olefin resin porous body, which limits its performance and applicability in applications such as battery separators.
By mixing the olefin-based resin with solvent in a pressure vessel, a polymer solution is formed and mixed with a high-pressure fluid of carbon dioxide, phase separation is caused by cooling, the formation of pore structure is controlled, and phase separation is adjusted using the temperature and solubility parameters of the high-pressure fluid. to form different types of pore structures.
The fine control of the pore structure of the olefin resin porous body is achieved, and the porous body with different structures can be manufactured. It is suitable for battery separators and other applications, and the battery resistance and mechanical strength are improved.
Smart Images

Figure CN116218064B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for producing an olefin-based resin porous body, and a method and apparatus for producing a battery separator. Background Art
[0002] Japanese Patent Application Laid-Open No. 2016-176061 discloses a porous sintered body made of polyethylene. Summary of the invention
[0003] Various olefin resin porous bodies (hereinafter may be simply referred to as "porous bodies") are manufactured. It is required to control the pore structure according to the application of the porous body.
[0004] The present disclosure discloses a method for producing an olefin-based resin porous body capable of controlling the pore structure.
[0005] The technical structure and effects of the present disclosure are described below. However, the mechanism of action in this specification includes assumptions. The mechanism of action does not limit the technical scope of the present disclosure.
[0006] 1. A method for producing an olefin-based resin porous body, comprising the following steps (a) to (f).
[0007] (a) An olefin resin and a solvent are mixed in a pressure vessel to prepare a polymer solution.
[0008] (b) Formation of high pressure fluids into carbon dioxide.
[0009] (c) Adjusting the temperature of the high pressure fluid.
[0010] (d) preparing a mixed fluid by mixing the temperature-controlled high-pressure fluid and the polymer solution in the pressure vessel.
[0011] (e) causing phase separation of the mixed fluid by cooling the mixed fluid.
[0012] (f) After the phase separation, the pressure in the pressure vessel is released to volatilize the solvent and carbon dioxide.
[0013] In the step (f), the solvent and carbon dioxide are volatilized to form an olefin-based resin porous body.
[0014] By mixing an olefin resin and a solvent, a polymer solution can be formed. 2 ) is mixed with the polymer solution. Thus, a mixed fluid is formed. In the mixed fluid, CO 2 It is a poor solvent. Phase separation is induced by cooling the mixed fluid. After phase separation, CO 2The solvent evaporates to form a porous body. The pore structure can change depending on the phase separation method.
[0015] According to the novel insights of the present disclosure, it is possible to pass high pressure fluid (CO 2 ) temperature to control the phase separation. It is believed that this is because the high-pressure fluid (CO 2 ) and the affinity of the polymer solution according to the high pressure fluid (CO 2 ) temperature.
[0016] 2. The olefin-based resin porous body may have at least one selected from the group consisting of a first pore structure, a second pore structure, and a third pore structure.
[0017] The first pore structure is formed by particles being linked together.
[0018] The second pore structure is a three-dimensional mesh structure. In the second pore structure, a plurality of bubble-like pores are interconnected.
[0019] The third pore structure is a three-dimensional mesh structure. In the third pore structure, a plurality of bubble-like pores are independent of each other.
[0020] In the manufacturing method of "1" above, for example, the first to third pore structures can be manufactured respectively. For example, the second pore structure is useful as a separator for a battery. Furthermore, for example, a porous body having both the first pore structure and the second pore structure can be formed. For example, a porous body having both the second pore structure and the third pore structure can be formed.
[0021] 3. The step (c) may include adjusting the temperature of the high-pressure fluid so that the phase separation becomes spinodal decomposition.
[0022] The phase separation mode can be controlled to spinodal decomposition by the temperature of the high-pressure fluid. It is considered that the second pore structure can be formed by spinodal decomposition.
[0023] 4. The step (c) may include adjusting the temperature of the high-pressure fluid so as to form a spinodal region in the liquid phase in a phase diagram between the polymer solution and the high-pressure fluid.
[0024] The phase diagram between the polymer solution and the high-pressure fluid can change depending on the temperature of the high-pressure fluid. This is probably because the affinity between the polymer solution and the high-pressure fluid changes depending on the temperature of the high-pressure fluid.
[0025] 5. In the spinodal region, the mixing ratio of the polymer solution and the high-pressure fluid can be adjusted.
[0026] The manner of phase separation can also be changed depending on the mixing ratio of the polymer solution and the high-pressure fluid.
[0027] 6. The step (c) may include adjusting the temperature of the high-pressure fluid so that the difference between the first solubility parameter of the olefin-based resin and the second solubility parameter of the high-pressure fluid becomes 5.3 or more.
[0028] There is a tendency that when the difference between the first solubility parameter of the olefin resin and the second solubility parameter of the high-pressure fluid is 5.3 or more, the second pore structure and the third pore structure are easily formed.
[0029] 7. The olefin resin may include polyethylene. In the step (c), the temperature of the high-pressure fluid may be adjusted to 50 to 100°C.
[0030] When the olefin resin includes polyethylene (PE), there is a tendency that the second pore structure and the third pore structure are easily formed when the temperature of the high-pressure fluid is 50 to 100°C.
[0031] 8. The olefin resin may include polypropylene. In the step (c), the temperature of the high-pressure fluid may be adjusted to 120 to 150°C.
[0032] When the olefin resin includes polypropylene (PP), the temperature of the high-pressure fluid passing therethrough is 120 to 150° C., and the second pore structure and the third pore structure tend to be easily formed.
[0033] 9. The above-mentioned high-pressure fluid may be a supercritical fluid.
[0034] 10. In the above step (f), before the pressure is released, the pressure container may be heated to 40-60°C.
[0035] 11. A method for producing a battery separator comprises the following steps (A) and (B).
[0036] (A) An olefin-based resin porous body is produced by using a method for producing an olefin-based resin porous body.
[0037] (B) Manufacturing a battery separator including the above-mentioned olefin-based resin porous body.
[0038] The olefin-based resin porous body can be used as, for example, a battery separator.
[0039] 12. The manufacturing device comprises a pressure vessel, a compression device, and a temperature adjustment device, wherein the pressure vessel seals the olefin resin and the solvent, the compression device compresses carbon dioxide to form a high-pressure fluid, and the temperature adjustment device adjusts the temperature of the high-pressure fluid. The manufacturing device is configured to: mix the olefin resin and the solvent in the pressure vessel to form a polymer solution, further mix the high-pressure fluid after temperature adjustment with the polymer solution in the pressure vessel, cool the mixed fluid formed by the high-pressure fluid and the polymer solution, and release the pressure in the pressure vessel after phase separation is achieved by cooling the mixed fluid.
[0040] The method for producing the olefin-based resin porous body described in the above-mentioned “1” can be carried out by using the production apparatus described in the above-mentioned “12”.
[0041] The following describes an embodiment of the present disclosure (hereinafter may be simply referred to as “the present embodiment”) and an example of the present disclosure (hereinafter may be simply referred to as “the present example”). However, the embodiment and the example do not limit the technical scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Features, advantages and technical and industrial significance of exemplary embodiments of the present invention will be described below with reference to the accompanying drawings, in which like numerals represent like elements, and in which:
[0043] Figure 1 This is a schematic flow chart of the method for producing the olefin-based resin porous body in the present embodiment.
[0044] Figure 2 This is a conceptual diagram showing an example of a production apparatus in this embodiment.
[0045] Figure 3 It is the phase diagram of polymer solution-high pressure flow system.
[0046] Figure 4 This is a phase diagram when the affinity between the polymer solution and the high-pressure fluid is high.
[0047] Figure 5 This is a phase diagram for the case where the affinity between a polymer solution and a high-pressure fluid is low.
[0048] Figure 6 This is a schematic flow chart of the method for producing the battery separator in this embodiment.
[0049] Figure 7 These are electron microscope images of the porous bodies of No. 1 to 4.
[0050] Figure 8 These are electron microscope images of the porous bodies of No. 5 to 8.
[0051] Fig. 9 These are electron microscope images of the porous bodies of No. 9 to 12. DETAILED DESCRIPTION
[0052] <Definitions of Terms, etc.>
[0053] In this specification, the descriptions of "having", "including", "having", and their variations (such as "consisting of...", etc.) are open forms. In addition to the essential elements, the open form may or may not contain additional elements. The description of "consisting of..." is a closed form. However, even in a closed form, usually incidental impurities and additional elements that are unrelated to the technology disclosed herein are not excluded. The description of "substantially consisting of..." is a semi-closed form. In the semi-closed form, the addition of elements that do not substantially affect the basic and novel characteristics of the technology disclosed herein is allowed.
[0054] In this specification, expressions such as “may perform…” and “can perform…” are not used in an obligatory sense (meaning “must perform…”) but in a permissive sense (meaning “has the possibility of performing…”).
[0055] In this specification, the multiple steps, actions and operations included in various methods are not limited to the order of recording unless otherwise specified. For example, multiple steps can also be performed simultaneously. For example, multiple steps can also be performed in reverse order.
[0056] In this specification, for example, a numerical range such as "m to n%" includes an upper limit and a lower limit unless otherwise specified. That is, "m to n%" means a numerical range of "more than m% and less than n%". In addition, "more than m% and less than n%" includes "more than m% and less than n%". Moreover, a numerical value arbitrarily selected from the numerical range may be used as a new upper limit or lower limit. For example, a new numerical range may be set by arbitrarily combining a numerical value within the numerical range with a numerical value recorded in another part, table, figure, etc. in this specification.
[0057] In this specification, all numerical values can be modified by the term "about". The term "about" can mean, for example, ±5%, ±3%, ±1%, etc. All numerical values can be approximate values that can vary according to the manner in which the disclosed technology is used. All numerical values can be represented by significant figures. The measured value can be an average value of several measurements. The number of measurements can be more than 3 times, more than 5 times, or more than 10 times. In general, the more measurements are made, the more reliable the average value can be expected to be. The measured value can be processed by rounding off based on the number of significant figures. The measured value can include, for example, errors associated with the detection limit of the measuring device.
[0058] The term "pressure container" as used herein refers to a sealed container that is subjected to pressure from at least one of the inside and the outside of the container. The pressure container may be configured to withstand a pressure of, for example, 0.2 to 50 MPa.
[0059] The "melting point" in this specification means the peak top temperature of the melting peak (endothermic peak) in the DSC (Differential Scanning Calorimetry) curve. The DSC curve can be measured in accordance with "JIS K 7121".
[0060] In this specification, "high-pressure fluid" means a fluid with a pressure above the critical pressure. High-pressure fluid includes supercritical fluid. "Supercritical fluid" means a fluid with a pressure above the critical pressure and a temperature above the critical temperature.
[0061] The term "olefin resin" as used herein refers to a polymer material synthesized from monomers containing chain olefins (alkene). The olefin resin may be a homopolymer or a copolymer. The olefin resin may include at least one selected from, for example, low-density polyethylene (LDPE), high-density polyethylene (HDPE), ultra-high molecular weight polyethylene (UHMW), polypropylene (PP), polymethylpentene (PMP: polymethylpentene) and ethylene-vinyl acetate copolymer (EVA: ethylene-vinyl acetate copolymer).
[0062] <Method for producing olefin-based resin porous body>
[0063] Figure 1 : is a schematic flow chart of the method for producing the olefin resin porous body in the present embodiment. Hereinafter, the "method for producing the olefin resin porous body in the present embodiment" may be referred to as "the present production method". The production method comprises the following steps: "(a) preparation of a polymer solution", "(b) formation of a high-pressure fluid", "(c) temperature adjustment", "(d) formation of a mixed fluid", "(e) phase separation", and "(f) release of pressure".
[0064] Manufacturing equipment
[0065] Figure 2: is a conceptual diagram showing an example of a manufacturing device in the present embodiment. Hereinafter, the "manufacturing device in the present embodiment" may be abbreviated as "the present manufacturing device". The present manufacturing device 100 may include, for example, a gas cylinder 1, a drying tube 2, a cooling device 3, a filter 4, a compression device 5, a first pressure gauge 6, a first safety valve 7, a temperature adjustment device 8, a check valve 9, a pressure vessel 10, a stirring device 11, a heating device 12, a second pressure gauge 13, a second safety valve 14, and a wet gas flow meter 15. Moreover, the present manufacturing device 100 may also include a back pressure valve 21, a first valve 22, a second valve 23, a third valve 24, etc. The first valve 22 to the third valve 24 can open and close the flow path independently. In the present manufacturing device 100, the present manufacturing method can be implemented.
[0066] (a) Preparation of polymer solution
[0067] The present production method includes the following steps: an olefin resin and a solvent are mixed in a pressure vessel 10 to prepare a polymer solution.
[0068] An olefin resin is prepared. For example, PE, PP, etc. may be prepared. The solvent may be, for example, a good solvent for the olefin resin. For example, the solvent may include n-pentane, etc.
[0069] An olefin resin and a solvent are put into a pressure vessel 10. The pressure vessel 10 is sealed. A polymer solution can be formed by mixing the olefin resin and the solvent in the pressure vessel 10. For example, the olefin resin and the solvent can be mixed by stirring the olefin resin and the solvent with a stirring device 11.
[0070] Generally, olefin resins tend to be difficult to dissolve in solvents. In order to promote solution formation, the olefin resin and the solvent may be mixed, for example, in a high temperature environment. For example, the olefin resin and the solvent may be mixed in a high temperature and high pressure environment. For example, the heating device 12 may heat the pressure vessel 10. The heating temperature may be, for example, the melting point of the olefin resin ± 20°C. The heating temperature may be, for example, 90 to 160°C.
[0071] For example, the polymer solution can be formed by dissolving an olefin resin in a solvent. For example, the polymer solution can be formed by mixing a melt of an olefin resin with a solvent.
[0072] The mixing ratio (ratio of the mass of the solvent to the mass of the olefin-based resin) may be, for example, 50 to 150, 50 to 100, or 100 to 150.
[0073] (b) Formation of high pressure fluid
[0074] The manufacturing method comprises the following steps: forming CO 2 For example, a high pressure fluid filled with CO 2Gas cylinder 1 supplies CO 2 .CO 2 The CO is supplied to the compression device 5 via the drying pipe 2 and the cooling device 3. The compression device 5 converts CO 2 Compressed to above critical pressure, thus forming a high-pressure fluid.
[0075] (c) Temperature adjustment
[0076] The manufacturing method comprises the following steps: adjusting the temperature of the high pressure fluid. In the manufacturing method, the high pressure fluid (CO 2 ) temperature to control the pore structure of the porous body.
[0077] For example, the temperature adjustment device 8 can adjust the temperature of the high-pressure fluid. The temperature adjustment device 8 can heat the high-pressure fluid or cool the high-pressure fluid. The temperature adjustment device 8 can include, for example, a preheating tube, a cooling tube, etc. The temperature adjustment device 8 can also include, for example, a pressure vessel, a stirring device, a heating device, etc. For example, the high-pressure fluid can be stirred and heated in the pressure vessel.
[0078] For example, the high-pressure fluid may be heated so that the temperature of the high-pressure fluid is above room temperature. For example, the high-pressure fluid may be heated so that the temperature of the high-pressure fluid exceeds 20° C. For example, the high-pressure fluid may be heated so that the temperature of the high-pressure fluid is above 30° C. For example, the high-pressure fluid may be heated so that the temperature of the high-pressure fluid is above 40° C. For example, the high-pressure fluid may be heated so that the temperature of the high-pressure fluid is above 50° C.
[0079] For example, the high-pressure fluid may be heated so that the temperature of the high-pressure fluid becomes equal to or higher than the critical temperature (31° C.) When the high-pressure fluid reaches the critical temperature or higher, a supercritical fluid can be formed.
[0080] (d) Formation of mixed fluid
[0081] The manufacturing method includes the following steps: a high-pressure fluid whose temperature has been adjusted is mixed with a polymer solution in a pressure vessel 10 to produce a mixed fluid.
[0082] By introducing the high-pressure fluid into the pressure container 10, the pressure in the pressure container 10 is pressurized. The pressure in the pressure container 10 is adjusted to 7.38 MPa (CO 2 The pressure in the pressure vessel 10 may also be adjusted to, for example, 10 to 20 MPa.
[0083] The mixed fluid is prepared by mixing the high pressure fluid and the polymer solution in the pressure container 10. For example, the stirring device 11 can stir the mixed fluid. 2 ) is a poor solvent.
[0084] (e) Phase separation
[0085] The manufacturing method includes the following steps: phase separation of the mixed fluid is caused by cooling the mixed fluid. For example, the pressure vessel 10 can be cooled by a water-cooled cooler (not shown). The temperature of the pressure vessel 10 is cooled to, for example, 15 to 25° C. After the temperature of the pressure vessel 10 reaches 15 to 25° C., the temperature of 15 to 25° C. is maintained for, for example, 20 to 40 minutes. Thus, phase separation of the mixed fluid is performed.
[0086] (f) Pressure release
[0087] The manufacturing method comprises the following steps: after phase separation, the pressure in the pressure vessel 10 is released to allow the solvent and CO to separate. 2 For example, before releasing the pressure, the heating device 12 may heat the pressure vessel 10 to 40-60° C. Before releasing the pressure, the generation of dry ice may be reduced by heating the pressure vessel 10. If dry ice is generated, there is a possibility that the pore structure may be damaged.
[0088] After the pressure vessel 10 is heated, the pressure vessel 10 is gradually depressurized. The depressurization time may be, for example, 10 to 30 minutes. During the depressurization process, the solvent and CO 2 The porous body is volatilized to form the porous body. The porous body can be recovered after the pressure vessel 10 reaches an equilibrium state. For example, the porous body can be recovered after the pressure vessel 10 reaches atmospheric pressure and room temperature (10 to 30° C.).
[0089] The porous body is manufactured by the above steps. The porous body can have any shape. The porous body can be, for example, in the form of a film, a block, or a sphere. When the porous body is in the form of a film, the porous body can have a thickness of, for example, 1 μm to 10 mm. The thickness of the porous body can be adjusted by, for example, the amount of olefin resin charged, the amount of solvent charged, and the area of the bottom surface in the pressure vessel 10.
[0090] Control of pore structure
[0091] In this production method, the pore structure of the porous body can be controlled.
[0092] Figure 3 is the phase diagram of polymer solution-high pressure flow system. Figures 3 to 5 In the above, "mass fraction of polymer solution" means the fraction of the mass of polymer solution relative to the total mass of polymer solution and high-pressure fluid. For example, when the mass fraction of polymer solution is 1, the system becomes a single phase of polymer solution. For example, when the mass fraction of polymer solution is 0 (zero), the system becomes a single phase of high-pressure fluid.
[0093] exist Figure 3 In the process of forming a solid, a mixed fluid (single-phase region) is cooled. By causing various phase separations during the formation of the solid, the pore structure can be controlled.
[0094] For example, the mixed fluid is cooled along the first line L1. The mixed fluid solidifies through the region sandwiched by the binodal and the spinodal. It is believed that nucleation-growth type decomposition occurs in this region. On the first line L1, the mass fraction of the polymer solution is low. That is, the high-pressure fluid (poor solvent) is relatively abundant. By preferentially performing nucleation of the polymer, a spherulite structure is formed. Thus, the first pore structure is formed. The first pore structure is formed by particle connection.
[0095] For example, the mixed fluid is cooled along the second line L2. The mixed fluid solidifies through the region (spinodal region) surrounded by the spinodal and the solidification line (crystallization temperature). It is believed that spinodal decomposition (liquid-liquid phase separation) is caused in the spinodal region. A modulated structure can be formed by spinodal decomposition. Thus, a second pore structure is formed. The second pore structure is a three-dimensional mesh. In the second pore structure, a plurality of bubble-like pores are interconnected. It is believed that the second pore structure is suitable for, for example, a battery separator.
[0096] For example, the mixed fluid is cooled along the third line L3. The mixed fluid solidifies through the region sandwiched by the binodal and the spinodal. It is believed that nucleation-growth type decomposition occurs in this region. On the third line L3, the mass fraction of the polymer solution is high. That is, there are relatively many polymers. An island structure is formed by preferentially performing nucleation of a poor solvent. Thus, a third pore structure is formed. The third pore structure is a three-dimensional mesh. In the third pore structure, a plurality of bubble-like pores are independent of each other. The third pore structure can be similar to the pore structure of a foam.
[0097] For example, the mixed fluid is cooled along the fourth line L4. The mixed fluid is solidified in a manner that does not intersect the binodal line. On the fourth line L4, the mass fraction of the polymer solution is the highest. Here, particle aggregates can be formed. The particle aggregates can have, for example, a cauliflower-like appearance.
[0098] For example, by adjusting the mixing ratio of the polymer solution and the high-pressure fluid in the spinodal region, the second pore structure can be selectively formed.
[0099] The phase diagram of the mixed system can be seen through the high pressure fluid (CO 2 ) is controlled by the temperature. It is believed that the affinity between the high-pressure fluid and the polymer solution changes depending on the temperature of the high-pressure fluid. The affinity can be evaluated using, for example, solubility parameters.
[0100] For example, the solubility parameter (δ 0) can be 14.2 (MPa) 0.5 For example, the first solubility parameter (δ 1 ) can be 16.3 (MPa) 0.5 It is considered that in the polymer solution, the olefin resin has a high affinity with the solvent.
[0101] For example, using 20°C, 15 MPa CO 2 As a high pressure fluid. CO 2 The second solubility parameter (δ 2 ) can be 14.2 (MPa) 0.5 Since the first solubility parameter (δ 1 ) and the second solubility parameter (δ 2 ) is small, so it is believed that in the mixed fluid, the polymer solution and the high-pressure fluid (CO 2 ) has a relatively high affinity.
[0102] Figure 4 This is a phase diagram when the affinity between the polymer solution and the high-pressure fluid is high. When the affinity between the polymer solution and the high-pressure fluid is high, the binodal and the spinodal are located on the low-temperature side of the solidification line. Therefore, liquid-liquid phase separation is not caused, but solid-liquid phase separation is caused. It is believed that the first pore structure (spherulite structure) is formed by solid-liquid phase separation.
[0103] For example, using 100°C, 15MPa CO 2 As a high pressure fluid. CO 2 The second solubility parameter (δ 2 ) can be 5.3 (MPa) 0.5 Since the first solubility parameter (δ 1 ) and the second solubility parameter (δ 2 ) is large, so it is believed that the polymer solution and the high-pressure fluid (CO 2 ) has a relatively low affinity.
[0104] Figure 5 This is a phase diagram for a case where the affinity between the polymer solution and the high-pressure fluid is low. As the affinity between the polymer solution and the high-pressure fluid becomes low, binodal lines and spinodal lines appear in the liquid phase domain. That is, a spinodal region is formed. It is believed that by causing liquid-liquid phase separation in the spinodal region, a second pore structure (modulated structure) can be formed. That is, by adjusting the temperature of the high-pressure fluid, a spinodal region can be formed in the liquid phase domain. By adjusting the temperature of the high-pressure fluid, phase separation can become spinodal decomposition.
[0105] Furthermore, through the high pressure fluid (CO 2) temperature rises, the solubility parameter decreases, it is believed that the density decreases with the temperature rise. For example, CO 2 (20℃, 15MPa) can have 903kg / m 3 For example, CO 2 (100°C, 15MPa) can have 332kg / m 3 density.
[0106] <Method for producing battery separator>
[0107] The porous body can be used for any purpose. For example, the porous body can be used as a battery separator (hereinafter simply referred to as a "separator").
[0108] Figure 6 : is a schematic flow chart of the method for producing a battery separator in the present embodiment. The method for producing a separator includes the following steps: "(A) producing a porous body" and "(B) producing a separator".
[0109] (A) Production of porous body
[0110] The manufacturing method of the separator comprises the following steps: a porous body is manufactured by using the manufacturing method. The details of the manufacturing method have been described above.
[0111] (B) Manufacturing of partitions
[0112] The method for manufacturing a partition includes the following steps: manufacturing a partition including a porous body. The partition is an electrically insulating porous film. For example, the partition can be manufactured by subjecting the porous body to various processes such as cutting, stretching, and compression. For example, when the porous body is in the form of a membrane, a multilayer partition can be manufactured by stacking a plurality of porous bodies. For example, the partition can be manufactured by coating a ceramic material on the surface of the porous body. The partition can have a thickness of, for example, 1 to 100 μm, and can have a thickness of 10 to 50 μm.
[0113] The separator may be a separator for a lithium ion battery, for example. The porous body may have, for example, a second pore structure (three-dimensional mesh, interconnected pores). When the porous body has the second pore structure, for example, a reduction in battery resistance may be expected.
[0114] The porous body may contain PE, for example. By containing PE in the porous body, for example, a shutdown function can be imparted to the separator. The so-called shutdown function is a function of blocking ion conduction by blocking pores when the battery temperature rises. The porous body may contain PP, for example. By containing PP in the porous body, mechanical strength, electrochemical stability, etc. can be imparted to the separator.
[0115] <Materials used>
[0116] In this example, the following materials were used.
[0117] Low-density polyethylene: Petrosen (registered trademark), manufactured by Toray Industries, Inc.
[0118] Level 353
[0119] Melt mass flow rate 145g / 10min
[0120] Density 915kg / m 3
[0121] Melting temperature 98℃
[0122] Homopolypropylene: Polypropylene (registered trademark), manufactured by Polypropylene Co., Ltd.
[0123] Grade J137G
[0124] Melt mass flow rate 30g / 10min
[0125] Density 915kg / m 3
[0126] n-Pentane: CAS No.109-66-0
[0127] <Production of olefin-based resin porous body>
[0128] The porous bodies Nos. 1 to 12 were produced as follows.
[0129] No.1
[0130] Prepared Figure 2 The present production apparatus 100. 0.06 g of PE (olefin resin) and 3.0 g of n-pentane (solvent) were sealed in the pressure vessel 10. The heating device 12 heated the pressure vessel 10 to 95°C.
[0131] Gas cylinder 1 supplies CO 2 (gas). CO is compressed by the compression device 5 2 The temperature control device 8 controls the temperature of the high pressure fluid to 20°C.
[0132] The temperature-controlled high-pressure fluid is introduced into the pressure vessel 10. The high-pressure fluid is supplied so that the pressure in the pressure vessel 10 becomes 15 MPa.
[0133] The water-cooled chiller cooled the pressure vessel 10 to 20° C. After reaching 20° C., the temperature near 20° C. was maintained for 30 minutes.
[0134] The heating device 12 heats the pressure vessel 10 to 50° C. After heating, the pressure vessel 10 is gradually depressurized. The depressurization time is 20 minutes.
[0135] The porous body is recovered when the pressure in the pressure container 10 reaches atmospheric pressure and room temperature. The porous body is manufactured through the above steps.
[0136] No.2~4
[0137] A porous body was produced in the same manner as in No. 1 except that the temperature of the high-pressure fluid was changed as shown in Table 1 below.
[0138] No.5~8
[0139] A porous body was produced in the same manner as in No. 1 except that the amount of material charged and the temperature of the high-pressure fluid were changed as shown in Table 1 below.
[0140] No.9~12
[0141] A porous body was produced in the same manner as in No. 1 except that the type of olefin resin, the amount of material charged, and the temperature of the high-pressure fluid were changed as shown in Table 1 below.
[0142]
[0143] <Results>
[0144] Figure 7 These are electron microscope images of the porous bodies of No. 1 to 4. In No. 1 to 4, it was observed that the high pressure fluid (CO 2 ) increases in temperature, the pore structure tends to change (see Table 1 above).
[0145] The porous body No. 1 has a first pore structure (refer to Figure 7 ). The first pore structure (spherulite structure) is formed by particles connecting.
[0146] The porous bodies of No. 2 and 3 have the second pore structure (refer to Figure 7 ). The second pore structure is a three-dimensional mesh. In the second pore structure, a plurality of bubble-like pores are interconnected. That is, the second pore structure includes interconnected pores. It is characterized in that the size of the bubble-like pores varies.
[0147] The porous body No. 4 has the third pore structure (refer to Figure 7 ). The third pore structure is a three-dimensional mesh. In the third pore structure, a plurality of bubble-like pores are independent of each other. That is, the third pore structure includes independent pores.
[0148] A 1.1 kg stainless steel (SUS) plate was placed on each of the porous bodies No. 1 to 4. After 20 seconds, the state of each porous body was visually confirmed. No. 1 (spherulite) could not maintain the film shape and disintegrated. It is believed that this is because the bonding between the particles is weak and brittle. No. 2 to No. 4 (mesh shape) maintained the film shape.
[0149] Figure 8 These are electron microscope images of the porous bodies No. 5 to 8. In the porous body No. 5, the characteristics of both the first pore structure and the second pore structure were observed (see Figure 8 ).
[0150] It was observed that the first solubility parameter (δ 1 ) and the second solubility parameter (δ 2 ) 1 -δ 2 ) is 5.3 (MPa) 0.5 When the above value is greater than 1.5, the second pore structure and the third pore structure tend to be easily formed (see Table 1 above).
[0151] When the olefin resin is PE, the difference in solubility parameters (δ 1 -δ 2 ) can be, for example, 6.8 (MPa) 0.5 The difference in solubility parameters (δ 1 -δ 2 ) can be, for example, 11 (MPa) 0.5 Below, it can be 8.7 (MPa) 0.5 the following.
[0152] When the olefin resin is PE, it is observed that the second pore structure and the third pore structure tend to be easily formed by adjusting the temperature of the high-pressure fluid to 50 to 100° C. (see Table 1 above).
[0153] When the olefin resin is PE, the temperature of the high-pressure fluid may be, for example, 60° C. or higher, or 65° C. or higher. When the olefin resin is PE, the temperature of the high-pressure fluid may be, for example, 75° C. or lower, or 70° C. or lower. It was observed that when the temperature of the high-pressure fluid was 75° C. or lower, the second pore structure tended to be easily formed (see Table 1 above).
[0154] Fig. 9 These are electron microscope images of porous bodies of Nos. 9 to 12. When the olefin resin is PP, it is observed that the second pore structure and the third pore structure tend to be easily formed by adjusting the temperature of the high-pressure fluid to 120 to 150°C (see Table 1 above).
[0155] When the olefin resin is PP, the temperature of the high-pressure fluid may be, for example, 130° C. or higher, or 140° C. or higher. It was observed that when the temperature of the high-pressure fluid is 130° C. or higher, the second pore structure tends to be easily formed (see Table 1 above). When the olefin resin is PP, the temperature of the high-pressure fluid may be, for example, 150° C. or lower.
[0156] When the olefin resin is PP, the difference in solubility parameters (δ 1 -δ 2 ) For example, it can be 13.9 to 14.3 (MPa) 0.5 .
[0157] The present embodiment and the present example are illustrative in all aspects. The present embodiment and the present example are not restrictive. The technical scope of the present disclosure includes all changes within the meaning and scope equivalent to the records of the claims. For example, it is presupposed from the beginning that any configuration can be extracted from the present embodiment and the present example and they can be combined arbitrarily.
Claims
1. A method for producing an olefin resin porous body, It is characterized in that The following steps are involved: (a) preparing a polymer solution by mixing an olefin resin and a solvent in a pressure vessel and heating the mixture to a temperature within ±20° C. of the melting point of the olefin resin; (b) compressing carbon dioxide to a pressure above the critical pressure to form a high-pressure fluid of carbon dioxide; (c) adjusting the temperature of the high pressure fluid; (d) preparing a mixed fluid by mixing the temperature-controlled high-pressure fluid with the polymer solution in the pressure vessel; (e) causing phase separation of the mixed fluid by cooling the mixed fluid; and (f) after the phase separation, volatilizing the solvent and carbon dioxide by releasing the pressure in the pressure vessel, wherein, in the step (f), the olefin resin porous body is formed by volatilizing the solvent and carbon dioxide; The step (c) includes adjusting the temperature of the high-pressure fluid so that the phase separation becomes spinodal decomposition.
2. The manufacturing method according to claim 1, It is characterized in that The olefin resin porous body has a second pore structure, The second pore structure is in a three-dimensional mesh shape, and a plurality of bubble-like pores are interconnected in the second pore structure.
3. The manufacturing method according to claim 1, It is characterized in that The step (c) includes adjusting the temperature of the high-pressure fluid so that a spinodal region is formed in a liquid phase in a phase diagram between the polymer solution and the high-pressure fluid.
4. The manufacturing method according to claim 3, It is characterized in that In the spinodal region, the mixing ratio of the polymer solution and the high-pressure fluid is adjusted.
5. The production method according to any one of claims 1 to 4, It is characterized in that The step (c) includes adjusting the temperature of the high-pressure fluid so that the difference between a first solubility parameter of the olefin-based resin and a second solubility parameter of the high-pressure fluid becomes 5.3 or more.
6. The manufacturing method according to claim 1, It is characterized in that The olefin resin comprises polyethylene, In the step (c), the temperature of the high-pressure fluid is adjusted to 50-100°C.
7. The manufacturing method according to claim 1, It is characterized in that The olefin-based resin includes polypropylene, In the step (c), the temperature of the high pressure fluid is adjusted to 120-150°C.
8. The production method according to any one of claims 1 to 4, It is characterized in that The high pressure fluid is a supercritical fluid.
9. The production method according to any one of claims 1 to 4, It is characterized in that In the step (f), the pressure vessel is heated to 40-60° C. before the pressure is released.
10. A method for manufacturing a separator for a battery, It is characterized in that The following steps are involved: (A) producing an olefin resin porous body by the production method according to any one of claims 1 to 9; and (B) producing a battery separator comprising the olefin-based resin porous body.
Citation Information
Patent Citations
Ultra-high molecular weight polyethylene-made porous sintered body
JP2016176061A
Method for preparing polypropylene resin foam particles through supercritical CO2 process
CN102924742A
Method for manufacturing foamed polypropylene-resin particles
CN105008443A
Method for producing porous olefin resin body
CN114805903A
Method for producing porous olefin resin body
CN114835939A