Polyethylene composition and preparation method thereof, polyethylene film and preparation method thereof
By adjusting the proportion of low-density and high-density polyethylene in polyethylene films and the melt flow rate ratio, a polyethylene film with excellent impact resistance was prepared, which solved the problem of insufficient impact resistance of films in the prior art, and realized the Better mechanical properties.
Patent Information
- Application Number
- CN202111491392.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-12-08
AI Technical Summary
The films made of existing polyethylene compositions have poor impact resistance and cannot effectively protect the integrity of contents with heavier mass under impact conditions.
Using a polyethylene composition including low-density polyethylene, low-density polyethylene and high-density polyethylene, a polyethylene film with excellent impact resistance is prepared by adjusting the density of components and the melt mass flow rate ratio. The specific method is to mix components A, component B and component C in proportion and then melt blend and granulate, and then prepare a film by extrusion and blowing traction. The thickness and blowing ratio of the film are between 20-70 μm and Between 2.0-3.0.
The impact strength, tensile and tear properties of polyethylene films have been significantly improved, and the impact damage quality, tensile strength and right-angle tear strength have reached a high level, which is suitable for protecting contents with heavier quality.
Smart Images

Figure BDA0003399511470000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyethylene, and in particular relates to a polyethylene composition and a preparation method thereof, a polyethylene film and a preparation method thereof. Background Art
[0002] In recent years, the packaging industry has developed rapidly. In addition to the basic protection function, packaging materials should be reasonably strengthened in terms of barrier properties, sealing properties, mechanical properties, etc. according to the characteristics of the contents and the quality assurance requirements. For heavier contents, the impact resistance of packaging is undoubtedly an important indicator related to product safety.
[0003] Impact resistance is one of the important mechanical properties of packaging film materials, reflecting the ability of the material to resist external destructive forces. Especially for packaging materials with small or no gaps between the packaging materials and the contents, and heavy packaging, impact resistance directly affects the integrity and protective function of the packaging under impact conditions, and can effectively avoid product damage during circulation due to poor impact resistance of packaging film materials. Therefore, reasonable and effective impact resistance is the key point of plastic packaging.
[0004] Chinese patent CN201710973431.X discloses a polyethylene composition and a film thereof, wherein the polyethylene composition contains component A, component B, component C and component D; component A is polypropylene, component B is low-density polyethylene, component C is linear low-density polyethylene, component D is an antioxidant, and based on the total content of the polyethylene composition, the content of polypropylene is 2-10 parts by weight, the content of low-density polyethylene is 20-45 parts by weight, the content of linear low-density polyethylene is 50-78 parts by weight, and the content of the antioxidant is 0.1-0.4 parts. The film has excellent properties of puncture resistance, good tensile and impact properties, low haze, and fewer crystal point fish eyes.
[0005] Chinese patent CN201911121008.2 discloses a polyethylene composition, polyethylene plastic particles prepared from the polyethylene composition, packaging products prepared from the polyethylene plastic particles, and the use of the packaging products in packaging volatile medicinal ingredients. The polyethylene composition provided by the present invention comprises polyethylene and organic molecules. The polyethylene plastic particles prepared from the polyethylene composition have good tensile properties, mechanical strength and appearance, and are suitable for preparing packaging products, especially blow-molded packaging products. In the present invention, organic molecules are added to the polyethylene composition, and when the polyethylene plastic particles prepared from the polyethylene composition are used to prepare packaging products, the organic molecules can play the role of "molecular placeholders", making it difficult for volatile medicinal ingredients to migrate out of the packaging products. However, the invention does not highlight excellent impact resistance. Summary of the invention
[0006] The object of the present invention is to provide a polyethylene composition to solve the problem that the film made of the polyethylene composition in the prior art has poor impact resistance.
[0007] The present invention also aims to provide a method for preparing a polyethylene composition, a polyethylene film and a method for preparing the same.
[0008] To achieve the above object, the present invention provides a polyethylene composition, comprising three components A, B, and C, wherein A and B are low-density polyethylene, C is high-density polyethylene, wherein -10.5≤M C / M B —M B / M A ≤10.0, where M A is the melt mass flow rate of component A, M B is the melt mass flow rate of component B, M C is the melt mass flow rate of component C.
[0009] The polyethylene composition of the present invention, wherein -5.0≤M C / M B —M B / M A ≤7.5, more preferably, -4.5≤M C / M B —M B / M A ≤6.0.
[0010] In the present invention, component A, component B and component C are all copolymers of ethylene and α-olefins, and the α-olefins in component A, component B and component C are each independently one of C3-C12 olefins. Preferably, the α-olefin is one of 1-butene, 1-hexene and 1-octene.
[0011] The polyethylene composition of the present invention, wherein the density of component A is in the range of 0.908-0.926 g / cm 3 , the density range of component B is 0.904-0.923g / cm 3 , the density range of component C is 0.940-0.960g / cm 3 .
[0012] The polyethylene composition of the present invention, wherein the density of component A is in the range of 0.912-0.921 g / cm 3 , the density range of component B is 0.910-0.918g / cm 3 , the density of component C is in the range of 0.944-0.950 g / cm 3 .
[0013] The polyethylene composition of the present invention, wherein the melt mass flow rate M of component A at 190°C and 2.16 kg is A The melt mass flow rate M of component B is in the range of 0.1-3.0 g / 10 min. B The melt mass flow rate M of component C is in the range of 0.8-6.0 g / 10 min. C The range is 5.0-20.0g / 10min.
[0014] The polyethylene composition of the present invention, wherein the melt mass flow rate M of component A at 190°C and 2.16 kg is A The melt mass flow rate M of component B is in the range of 0.2-0.6 g / 10 min. B The melt mass flow rate M of component C is in the range of 1.0-3.0 g / 10 min. C The range is 9.0-12.0g / 10min.
[0015] The polyethylene composition of the present invention comprises 60-80 parts of component A, 10-25 parts of component B and 5-15 parts of component C based on 100 parts of the total weight of the composition.
[0016] To achieve the above object, the present invention also provides a method for preparing a polyethylene composition, comprising melt blending and granulating a mixture of component A, component B and component C in proportion, and the extrusion temperature is 180-220°C.
[0017] To achieve the above object, the present invention also provides a polyethylene film prepared from the polyethylene composition, wherein the film has a thickness of 20-70 μm, preferably 40-60 μm.
[0018] To achieve the above object, the present invention also provides a method for preparing a polyethylene film, wherein the polyethylene composition prepared according to the above method is extruded, blown and drawn, and the extrusion temperature is 190-260°C, preferably 220-245°C.
[0019] The method for preparing the polyethylene film of the present invention, wherein the blowing ratio is 2.0-3.0, preferably 2.5-3.0.
[0020] The beneficial effects of the present invention are:
[0021] When the polyethylene composition of component A, component B and component C having the above-mentioned specific density and melt mass flow rate is prepared into a film, the film has good tensile properties and tear properties, and outstandingly, has a good effect on impact strength. DETAILED DESCRIPTION
[0022] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.
[0023] The polyethylene composition and the corresponding polyethylene composition film are prepared by mechanically mixing component A, component B, component C and an auxiliary agent in proportion, and then extruding them into particles using a ZSK25 twin-screw extruder (model ZSK-25P8.2E, manufactured by Coperion, Germany); and the obtained polyethylene composition particles are made into polyethylene films using a vertical film blowing machine (model SJ-45*25-FM600, manufactured by Dalian Rubber and Plastic Machinery Factory).
[0024] The impact damage quality of the film is measured according to the method specified in GB 9639.1-2008; the tensile strength is measured according to the method specified in GB / T1040.3-2006; and the right-angle tear strength is measured according to the method specified in GB / T 16578.2-2009.
[0025] Example 1
[0026] Component A is commercially available low-density polyethylene with a density of 0.916 g / cm 3 , melt mass flow rate M A Component B is commercially available low-density polyethylene with a density of 0.918 g / cm 3 , melt mass flow rate M B 1.0g / 10min; Component C is commercially available high-density polyethylene with a density of 0.949g / cm 3 , melt mass flow rate M C The relationship between the melt mass flow rates of component A, component B and component C is: C / M B —M B / M A =6.0, satisfying -5.0≤M C / M B —M B / M A ≤7.5.
[0027] Based on the total weight of the polyethylene composition of 100 parts, the weight of component A is 60 parts, the weight of component B is 25 parts, and the weight of component C is 15 parts. The components are weighed in proportion and mixed, and extruded and granulated using a ZSK25 twin-screw extruder to obtain polyethylene composition pellets.
[0028] The polyethylene composition pellets prepared above were added into a SJ-45*25-FM600 vertical film blowing machine, and the extrusion screw temperature was 220° C. to obtain a polyethylene composition film with a film thickness of 60 μm and a blow-up ratio of 2.5.
[0029] Example 2
[0030] Component A is commercially available low-density polyethylene with a density of 0.916 g / cm 3 , melt mass flow rate M A Component B is commercially available low-density polyethylene with a density of 0.918 g / cm 3 , melt mass flow rate M B Component C is commercially available high-density polyethylene with a density of 0.949 g / cm 3 , melt mass flow rate M C The relationship between the melt mass flow rates of component A, component B and component C is: C / M B —M B / M A =-4.5, satisfying -5.0≤M C / M B —M B / M A ≤7.5.
[0031] Based on the total weight of the polyethylene composition of 100 parts, the weight of component A is 60 parts, the weight of component B is 25 parts, and the weight of component C is 15 parts. The components are weighed in proportion and mixed, and extruded and granulated using a ZSK25 twin-screw extruder to obtain polyethylene composition pellets.
[0032] The polyethylene composition pellets prepared above were added into a SJ-45*25-FM600 vertical film blowing machine, and the extrusion screw temperature was 220° C. to obtain a polyethylene composition film with a film thickness of 60 μm and a blow-up ratio of 2.5.
[0033] Example 3
[0034] Component A is commercially available low-density polyethylene with a density of 0.921 g / cm 3 , melt mass flow rate M A Component B is commercially available low-density polyethylene with a density of 0.918 g / cm 3 , melt mass flow rate M B 1.0g / 10min; Component C is commercially available high-density polyethylene with a density of 0.949g / cm 3 , melt mass flow rate M CThe relationship between the melt mass flow rates of component A, component B and component C is: C / M B —M B / M A =7, satisfying -5.0≤M C / M B —M B / M A ≤7.5.
[0035] Based on the total weight of the polyethylene composition of 100 parts, the weight of component A is 60 parts, the weight of component B is 25 parts, and the weight of component C is 15 parts. The components are weighed in proportion and mixed, and extruded and granulated using a ZSK25 twin-screw extruder to obtain polyethylene composition pellets.
[0036] The polyethylene composition pellets prepared above were added into a SJ-45*25-FM600 vertical film blowing machine, and the extrusion screw temperature was 220° C. to obtain a polyethylene composition film with a film thickness of 60 μm and a blow-up ratio of 2.5.
[0037] Example 4
[0038] The component composition, polyethylene composition and polyethylene film were prepared in the same manner as in Example 1, except that the mass fractions of the components were changed so that the mass of component A was 65 parts, the mass of component B was 20 parts, and the mass of component C was 15 parts.
[0039] Example 5
[0040] The component composition, polyethylene composition and polyethylene film were prepared in the same manner as in Example 2, except that the mass fractions of the components were changed so that the mass of component A was 70 parts, the mass of component B was 20 parts, and the mass of component C was 10 parts.
[0041] Example 6
[0042] The component composition, polyethylene composition and polyethylene film were prepared in the same manner as in Example 3, except that the mass fractions of the components were changed so that the mass of component A was 75 parts, the mass of component B was 15 parts, and the mass of component C was 10 parts.
[0043] Example 7
[0044] The component composition, the mass fraction of each component and the preparation method of the polyethylene composition are the same as those in Example 1. The thickness of the prepared polyethylene film is 50 μm and the blowing ratio is 3.0.
[0045] Example 8
[0046] The component composition, mass fraction of each component and preparation method of the polyethylene composition were the same as those in Example 2. The thickness of the prepared polyethylene film was 40 μm and the blowing ratio was 3.0.
[0047] Example 9
[0048] The component composition, the mass fraction of each component and the preparation method of the polyethylene composition are the same as those in Example 3. The thickness of the prepared polyethylene film is 50 μm and the blowing ratio is 2.5.
[0049] Comparative Example 1
[0050] The polyethylene film was prepared in the same manner as in Example 1, except that component A and component B in Example 1 were removed and only component C was retained, and then a polyethylene film was prepared.
[0051] Comparative Example 2
[0052] The method for preparing the polyethylene film is the same as that in Example 1, except that component C in Example 1 is removed, and the mass fraction of the retained component A is 50 parts, and the mass fraction of the retained component B is 50 parts, and then a polyethylene film is prepared.
[0053] Comparative Example 3
[0054] The component composition, polyethylene composition and polyethylene film were prepared in the same manner as in Example 2, except that the mass fractions of each component were changed so that the mass of component A was 25 parts, the mass of component B was 25 parts, and the mass of component C was 50 parts.
[0055] Comparative Example 4
[0056] Component A is commercially available low-density polyethylene with a density of 0.916 g / cm 3 , melt mass flow rate M A Component B is commercially available low-density polyethylene with a density of 0.918 g / cm 3 , melt mass flow rate M B 3.0g / 10min; Component C is commercially available high-density polyethylene with a density of 0.949g / cm 3 , melt mass flow rate M C The relationship between the melt mass flow rates of component A, component B and component C is: C / M B —M B / M A =-11.3.
[0057] The polyethylene films obtained in the above examples and comparative examples were subjected to performance tests, and the test items included impact damage mass, tensile strength and right-angle tear strength. The results are shown in Table 1.
[0058] Table 1 Test results of mechanical properties of polyethylene film
[0059]
[0060] By analyzing the film performance test results of the embodiments and comparative examples in Table 1, it can be seen that the film prepared from the polyethylene composition provided in the present invention has high impact damage mass, tear strength and tensile strength. Impact damage mass ≥ 400g, longitudinal tensile strength ≥ 50MPa, transverse tensile strength ≥ 45MPa, right-angle tear strength ≥ 120kN / m. When the melt mass flow rate of each component in the polyethylene composition satisfies -5.0≤M C / M B —M B / M A When ≤7.5, the impact damage quality, tear strength and tensile strength of the film in Examples 1-9 are improved compared with those in Comparative Examples 1-4.
[0061] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A polyethylene composition comprising three components A, B and C, wherein: A and B are low-density polyethylene, C is high-density polyethylene, characterized in that -4.5 ≤ M C / M B —M B / M A ≤ 7.0, where M A is the melt mass flow rate of component A, M B is the melt mass flow rate of component B, M C is the melt mass flow rate of component C; The density of component A ranges from 0.912 to 0.921 g / cm 3 , the density range of component B is 0.910-0.918g / cm 3 , the density of component C is in the range of 0.944-0.950 g / cm 3 ; At 190°C and 2.16 kg, the melt mass flow rate M of component A is A The melt mass flow rate M of component B is in the range of 0.1-3.0 g / 10 min. B The melt mass flow rate M of component C is in the range of 0.8-6.0 g / 10 min. C The range is 5.0-20.0 g / 10 min; Based on 100 parts by total weight of the composition, the composition comprises 60-80 parts of component A, 10-25 parts of component B and 5-15 parts of component C.
2. The polyethylene composition according to claim 1, characterized in that At 190°C and 2.16 kg, the melt mass flow rate M of component A is A The melt mass flow rate M of component B is in the range of 0.2-0.6 g / 10 min. B The melt mass flow rate M of component C is in the range of 1.0-3.0 g / 10 min. C The range is 9.0-12.0g / 10min.
3. The method for preparing the polyethylene composition according to any one of claims 1 to 2, characterized in that: The mixture of component A, component B and component C in proportion is melt-blended and granulated, and the extrusion temperature is 180-220°C.
4. A polyethylene film prepared from the polyethylene composition according to any one of claims 1 to 2, characterized in that: The film thickness is 20-70μm.
5. The polyethylene film according to claim 4, characterized in that: The film thickness is 40-60μm.
6. The method for preparing the polyethylene film according to claim 4, characterized in that: The polyethylene composition prepared according to the method of claim 3 is extruded, blown and drawn, and the extrusion temperature is 190-260°C.
7. The method for preparing a polyethylene film according to claim 6, characterized in that: The extrusion temperature is 220-245°C.
8. The method for preparing a polyethylene film according to claim 6, characterized in that: The blowing ratio is 2.0-3.
0.