Surface-coated modified metal powder material and preparation method thereof, and microwave absorbing material
By coating the surface of metal particles with polydopamine and calcining it to form a carbon skeleton structure, combined with ZIF-67 composite material, the problem of insufficient performance of existing absorbing materials is solved, and a comprehensive improvement in absorbing strength, frequency band width and density thickness is achieved. Suitable for electromagnetic stealth and jamming applications.
Patent Information
- Application Number
- CN202111516303.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-07
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-12-07
AI Technical Summary
Existing absorbing materials cannot take into account good absorbing strength, wide absorbing frequency band, thin thickness and low density, which limits their application in practical applications.
By coating the surface of metal particles with polydopamine and calcining in an inert atmosphere to form a metal/porous carbon structure with carbon as the skeleton, combined with ZIF-67 composite material, a composite material with high absorbing strength, wide frequency band, low density and thin Thickness of absorbing material.
The comprehensive performance improvement of the absorbing material has been achieved, and it has the characteristics of high absorbing intensity, wide frequency band, low density and thin thickness, and is suitable for electromagnetic stealth and interference applications.
Smart Images

Figure BDA0003397052660000071
Abstract
Description
Technical Field
[0001] The present invention relates to the field of wave-absorbing materials, and in particular to a surface-coated modified metal powder material and a preparation method thereof, and a wave-absorbing material. Background Art
[0002] With the development of electromagnetic stealth technology in the military field and the increasingly serious problems of electromagnetic interference and electromagnetic pollution, microwave absorbing materials have gradually become a research hotspot in the field of functional materials. Traditional absorbing materials, such as ferrite, metal powder and silicon carbide, usually have shortcomings such as narrow absorption band, high density and large filling ratio, which limits their application in practice. In practical applications, ideal absorbing materials need to meet the requirements of thin thickness, light weight, wide absorption band and strong absorption performance ("thin, light, wide and strong"). Therefore, the development of new absorbing materials with novel structure and excellent comprehensive performance has important scientific value and application prospects. Summary of the invention
[0003] The main purpose of the present invention is to provide a surface-coated modified metal powder material and a preparation method thereof, and an absorbing material to solve the problem that the absorbing materials in the prior art cannot take into account good absorbing strength, a wider absorbing frequency band, a thinner thickness and a lower density.
[0004] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a method for preparing a surface-coated modified metal powder material, which comprises: step S1, coating polydopamine on the surface of metal particles to form polydopamine-coated powder; step S2, mixing a cobalt source, polydopamine-coated powder, 2-methylimidazole and a solvent, and then reacting to form a reaction slurry; separating the reaction slurry from the solid and liquid, and drying it to obtain a precursor material; step S3, calcining the precursor material in an inert atmosphere to obtain a surface-coated modified metal powder material.
[0005] Furthermore, the metal particles are one or more of carbonyl iron powder, nickel powder, and sendust alloy powder; preferably, the metal particles are flaky metal powder with a thickness of 0.5 to 2 μm and a radial size of 2 to 100 μm.
[0006] Further, the cobalt source is Co(NO3)2·6H2O.
[0007] Furthermore, step S1 comprises: mixing metal particles and a dopamine aqueous solution, and performing an in-situ polymerization reaction under stirring to obtain a polydopamine-coated powder; preferably, the mass concentration of the dopamine aqueous solution is 1 to 5 mg / ml; preferably, 0.5 to 5 mg of metal particles are added to each milliliter of the dopamine aqueous solution; preferably, during the in-situ polymerization reaction, the pH value is 7.8 to 8.8; preferably, the temperature of the in-situ polymerization reaction is 20 to 40°C, and the time is 12 to 24 hours.
[0008] Furthermore, the weight ratio of the cobalt source to the polydopamine-coated powder is (1.4-2.2):(0.5-1.5); preferably, the weight ratio of 2-methylimidazole to the cobalt source is (1.6-2.2):(1.4-2.2).
[0009] Furthermore, step S2 includes: dividing the solvent into at least three parts, mixing the cobalt source with the first part of the solvent to form a first mixed liquid; dispersing the polydopamine-coated powder in the second part of the solvent to form a second mixed liquid; mixing 2-methylimidazole with the third part of the solvent to form a third mixed liquid; mixing the first mixed liquid with the second mixed liquid and stirring to form a pre-reaction liquid; mixing the pre-reaction liquid with the third mixed liquid, and reacting under stirring to form a reaction slurry; after centrifuging the reaction slurry, centrifugally washing and drying the precipitate to obtain a precursor material.
[0010] Furthermore, the solvent is an alcohol solvent; preferably, the solvent is methanol; preferably, after the first mixed liquid and the second mixed liquid are mixed, they are magnetically stirred for 1 to 3 hours to form a pre-reaction liquid; preferably, after the pre-reaction liquid and the third mixed liquid are mixed, they are magnetically stirred for 12 to 24 hours at a temperature of 20 to 40° C. to react and obtain a reaction slurry.
[0011] Furthermore, in step S3, during the calcination of the precursor material, the calcination temperature is 500-900° C., and the calcination time is 2-5 hours.
[0012] According to another aspect of the present invention, a surface-coated and modified metal powder material is provided, which is prepared by the above-mentioned preparation method.
[0013] According to another aspect of the present invention, there is also provided a wave absorbing material, which comprises the above-mentioned surface-coated modified metal powder material.
[0014] By using the preparation method of the present invention, metal particles are first coated with polydopamine (PDA), which not only allows the metal particles to be evenly dispersed in the solution, thereby improving the structural uniformity of the final powder material, but also allows polydopamine to form a carbon skeleton structure coated on the surface of the metal particles after subsequent high-temperature carbonization; in addition, the carbon skeleton structure formed by polydopamine as a coating layer can also isolate the metal from the air, thereby improving the chemical stability of the metal, such as oxidation resistance and corrosion resistance. More importantly, active anions exist on the surface of polydopamine, which can provide reaction sites for metal cations (cobalt) in the synthesis process of step S2, in which the cobalt source and 2-methylimidazole can react to form ZIF-67 and compound on the surface of polydopamine. Secondly, with calcination in an inert atmosphere, polydopamine is thermally decomposed into a carbon skeleton. ZIF-67 can also form cobalt or cobalt oxide particles after calcination and thermal decomposition and are evenly embedded in the carbon skeleton, forming a modified powder with a metal / porous carbon structure with carbon as the skeleton. It has a synergistic absorption mechanism of multiple losses such as dielectric loss, conductivity loss, and magnetic loss. Therefore, it has a higher absorption intensity and a wider absorption frequency band. At the same time, the material also has the characteristics of low density and relatively thin thickness. In short, it is an absorbing material with better comprehensive performance. DETAILED DESCRIPTION
[0015] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0016] As described in the background technology section, the absorbing materials in the prior art cannot take into account good absorbing strength, wide absorbing frequency band, thin thickness and low density. In order to solve the above problems, the present invention provides a method for preparing a surface-coated modified metal powder material, which comprises: step S1, coating polydopamine on the surface of metal particles to form polydopamine-coated powder; step S2, mixing a cobalt source, polydopamine-coated powder, 2-methylimidazole and a solvent, and then reacting to form a reaction slurry; separating the reaction slurry from solid and liquid, and drying to obtain a precursor material; step S3, calcining the precursor material in an inert atmosphere to obtain a surface-coated modified metal powder material.
[0017] Metal-Organic Frameworks (MOFs) are porous carbon composite materials with nanopores and open channel structures, which can be prepared by pyrolysis and uniformly embedded metal or metal oxide nanoparticles. The present invention uses a simple solvent method to coat and modify metal particles and composite them with porous MOFs (ZIF-67) to prepare a broadband, high-absorption, thin-thickness, light-density electromagnetic wave absorbing material.
[0018] Specifically, the present invention first coats the metal particles with polydopamine (PDA), which not only allows the metal particles to be evenly dispersed in the solution to improve the structural uniformity of the final powder material, but also allows the polydopamine to form a carbon skeleton structure coated on the surface of the metal particles after subsequent high-temperature carbonization; in addition, the carbon skeleton structure formed by polydopamine as a coating layer can also isolate the metal from the air, thereby improving the chemical stability of the metal, such as oxidation resistance and corrosion resistance. More importantly, there are active anions on the surface of polydopamine, which can provide reaction sites for metal cations (cobalt) during the synthesis process of step S2, in which the cobalt source and 2-methylimidazole can react to form ZIF-67 and compound on the surface of polydopamine. Secondly, with calcination in an inert atmosphere, polydopamine is thermally decomposed into a carbon skeleton. ZIF-67 can also form cobalt or cobalt oxide particles after calcination and thermal decomposition and are evenly embedded in the carbon skeleton, forming a modified powder with a metal / porous carbon structure (3D network framework structure) with carbon as the skeleton. It has a synergistic absorption mechanism of multiple losses such as dielectric loss (porous carbon can improve attenuation and dielectric loss, and the carbon skeleton coating layer can also improve dielectric loss), conductivity loss (carbon skeleton coating layer can improve conductivity loss), and magnetic loss (metal can improve magnetic loss). Therefore, it has a higher absorption intensity and a wider absorption band. At the same time, the material also has the characteristics of low density and relatively thin thickness. In short, it is an absorbing material with better comprehensive performance.
[0019] In a preferred embodiment, the metal particles are one or more of carbonyl iron powder, nickel powder, and iron-silicon-aluminum alloy powder; preferably, the metal particles are flaky metal powders with a thickness of 0.5 to 2 μm and a radial dimension (width perpendicular to the thickness direction) of 2 to 100 μm. The above types of metal particles are selected, on the one hand, to be more conducive to the coating of dopamine, thereby facilitating the improvement of the structural stability of the final powder material, and on the other hand, they cooperate with the carbon skeleton coating layer and the metal-organic framework material after the ZIF-67 composite, and have a more beneficial comprehensive wave absorption effect.
[0020] The above cobalt source can react with 2-methylimidazole in a solution to form a ZIF-67 material. In order to further improve the efficiency of the reaction and reduce the introduction of other impurity elements, in a preferred embodiment, the cobalt source is Co(NO3)2·6H2O.
[0021] In a preferred embodiment, step S1 comprises: mixing metal particles and a dopamine aqueous solution, and performing an in-situ polymerization reaction under stirring to obtain a polydopamine-coated powder. A polydopamine coating layer is formed on the surface of the metal particles by in-situ polymerization of dopamine under stirring, and the coating layer has a more uniform thickness and a more complete structure, which also has a better promoting and improving effect on the overall performance of the final material.
[0022] In order to make the coating more uniform and the thickness more suitable, preferably, the mass concentration of the dopamine aqueous solution is 1-5 mg / ml; preferably, 0.5-5 mg of metal particles are added to each ml of the dopamine aqueous solution. After the specific in-situ polymerization reaction, centrifugal separation can be performed first, and then the precipitate can be dried in a vacuum oven at 60-80°C for 12 hours to obtain polydopamine coated powder.
[0023] To make the in-situ polymerization reaction more complete, preferably, during the in-situ polymerization reaction, the pH value is 7.8-8.8 (such as 7.8, 8.0, 8.5, 8.8, etc.); preferably, the temperature of the in-situ polymerization reaction is 20-40° C., and the time is 12-24 hours.
[0024] In a preferred embodiment, the weight ratio of the cobalt source to the polydopamine-coated powder is (1.4-2.2):(0.5-1.5); preferably, the weight ratio of 2-methylimidazole to the cobalt source is (1.6-2.2):(1.4-2.2). The amount of the cobalt source and 2-methylimidazole is controlled within the above range. On the one hand, the two can react more fully to form ZIF-67, and on the other hand, the total amount is more suitable, so that the composite amount of cobalt metal or metal oxide particles in the final powder is more suitable, which has a better improvement on the overall performance of the absorbing material.
[0025] In order to make the reaction process more stable and to make ZIF-67 more stably generated at the anionic active center of the polydopamine coating layer, in a preferred embodiment, the above step S2 includes: dividing the solvent into at least three parts, mixing the cobalt source with the first part of the solvent to form a first mixed solution; dispersing the polydopamine-coated powder in the second part of the solvent to form a second mixed solution; mixing 2-methylimidazole with the third part of the solvent to form a third mixed solution; mixing the first mixed solution with the second mixed solution and stirring to form a pre-reaction solution; mixing the pre-reaction solution with the third mixed solution and reacting under stirring to form a reaction slurry; after centrifuging the reaction slurry, centrifugally washing and drying the precipitate to obtain a precursor material.
[0026] In a preferred embodiment, the solvent is an alcohol solvent; the preferred solvent is methanol. The selection of the above solvents can provide a more stable environment for the reaction of ZIF-67, and the polydopamine-coated particles can also form a good dispersion, which has a better promoting effect on improving the overall structural uniformity and performance uniformity of the material. Preferably, after the first mixed solution and the second mixed solution are mixed, magnetic stirring is performed for 1 to 3 hours to form a pre-reaction liquid; preferably, after the pre-reaction liquid and the third mixed solution are mixed, magnetic stirring is performed for 12 to 24 hours at a temperature of 20 to 40°C to react to obtain a reaction slurry. Specifically, after obtaining the reaction slurry, the centrifuged precipitate is centrifuged and washed 3 to 5 times with methanol, and then placed in a vacuum oven and dried at 60 to 80°C for 12 hours to obtain a precursor material.
[0027] In order to make polydopamine and ZIF-67 pyrolyze more fully to form a carbon skeleton and a porous carbon / metal composite material, in a preferred embodiment, in the above step S3, during the calcination of the precursor material, the calcination temperature is 500-900°C and the calcination time is 2-5h. In the specific calcination process, it is preferred to heat the precursor material from room temperature to the calcination temperature at a heating rate of 5°C / min and keep it for 2-5h to obtain the above modified metal powder material. The inert atmosphere during the calcination process includes but is not limited to nitrogen or argon.
[0028] According to another aspect of the present invention, a surface-coated and modified metal powder material is provided, which is prepared by the above-mentioned preparation method.
[0029] According to another aspect of the present invention, there is provided a wave absorbing material, which comprises the above-mentioned surface-coated modified metal powder material.
[0030] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0031] Example 1
[0032] (1) Ball-milled carbonyl iron powder (0.5 μm thick, radial size 10-50 μm) was added at 0.5 mg / ml into 100 ml of dopamine aqueous solution, wherein the concentration of the dopamine aqueous solution was 1 mg / ml, pH = 8.5, and magnetic stirring was performed at 25°C for 12 h. The mixture was then centrifuged and washed, and dried in a vacuum oven at 60°C for 12 h to obtain polydopamine-coated powder.
[0033] (2) 1.455 g Co(NO3)2·6H2O, 50 mg polydopamine-coated powder and 1.642 g 2-methylimidazole were dissolved in 100 ml, 150 ml and 100 ml methanol, respectively, and named as solution A, solution B and solution C. AB were first mixed and magnetically stirred for 1 h, then solution C was added to the AB mixture, magnetically stirred at room temperature for 12 h, centrifuged and washed 3 to 5 times with methanol centrifugation to obtain the product and dried in a vacuum oven at 60 ° C for 12 h to obtain the precursor material.
[0034] (3) The precursor material is heated to 900°C in a high-temperature furnace with nitrogen or argon as protective gas at a heating rate of 5°C / min and calcined for 2 h to obtain the final sample FeCo@C.
[0035] Example 2
[0036] (1) Ball-milled carbonyl iron powder (1 μm thick, radial size 10-50 μm) was added at 0.5 mg / ml into 100 ml of dopamine aqueous solution, wherein the concentration of the dopamine aqueous solution was 1 mg / ml, pH = 8.5, and magnetic stirring was performed at 25°C for 12 h. The mixture was then centrifuged and washed, and dried in a vacuum oven at 60°C for 12 h to obtain polydopamine-coated powder.
[0037] (2) 1.455 g Co(NO3)2·6H2O, 50 mg polydopamine-coated powder and 1.642 g 2-methylimidazole were dissolved in 100 ml, 150 ml and 100 ml methanol, respectively, and named as solution A, solution B and solution C. AB were first mixed and magnetically stirred for 1 h, then solution C was added to the AB mixture, magnetically stirred at room temperature for 12 h, centrifuged and washed 3 to 5 times with methanol centrifugation to obtain the product and dried in a vacuum oven at 60 ° C for 12 h to obtain the precursor material.
[0038] (3) The precursor material is heated to 900°C in a high-temperature furnace with nitrogen or argon as protective gas at a heating rate of 5°C / min and calcined for 2 h to obtain the final sample FeCo@C.
[0039] Example 3
[0040] (1) Ball-milled carbonyl iron powder (1.5 μm thick, radial size 10-50 μm) was added at 0.5 mg / ml into 100 ml of dopamine aqueous solution, wherein the concentration of the dopamine aqueous solution was 1 mg / ml, pH = 8.5, and magnetic stirring was performed at 25°C for 12 h. The mixture was then centrifuged and washed, and dried in a vacuum oven at 60°C for 12 h to obtain polydopamine-coated powder.
[0041] (2) 1.455 g Co(NO3)2·6H2O, 50 mg polydopamine-coated powder and 1.642 g 2-methylimidazole were dissolved in 100 ml, 150 ml and 100 ml methanol, respectively, and named as solution A, solution B and solution C. AB were first mixed and magnetically stirred for 1 h, then solution C was added to the AB mixture, magnetically stirred at room temperature for 12 h, centrifuged and washed 3 to 5 times with methanol centrifugation to obtain the product and dried in a vacuum oven at 60 ° C for 12 h to obtain the precursor material.
[0042] (3) The precursor material is heated to 900°C in a high-temperature furnace with nitrogen or argon as protective gas at a heating rate of 5°C / min and calcined for 2 h to obtain the final sample FeCo@C.
[0043] Example 4
[0044] (1) Ball-milled carbonyl iron powder (0.5 μm thick, radial size 10-50 μm) was added at 0.5 mg / ml into 100 ml of dopamine aqueous solution, wherein the concentration of the dopamine aqueous solution was 1 mg / ml, pH = 8.5, and magnetic stirring was performed at 25°C for 12 h. The mixture was then centrifuged and washed, and dried in a vacuum oven at 60°C for 12 h to obtain polydopamine-coated powder.
[0045] (2) 1.455 g Co(NO3)2·6H2O, 50 mg polydopamine-coated powder and 1.642 g 2-methylimidazole were dissolved in 100 ml, 150 ml and 100 ml methanol, respectively, and named as solution A, solution B and solution C. AB were first mixed and magnetically stirred for 1 h, then solution C was added to the AB mixture, magnetically stirred at room temperature for 12 h, centrifuged and washed 3 to 5 times with methanol centrifugation to obtain the product and dried in a vacuum oven at 60 ° C for 12 h to obtain the precursor material.
[0046] (3) The precursor material is heated to 600°C in a high-temperature furnace with nitrogen or argon as protective gas at a heating rate of 5°C / min and calcined for 2 h to obtain the final sample FeCo@C.
[0047] Example 5
[0048] (1) Ball-milled carbonyl iron powder (0.5 μm thick, radial size 10-50 μm) was added at 5 mg / ml into 100 ml of dopamine aqueous solution, wherein the concentration of the dopamine aqueous solution was 1 mg / ml, pH = 8.8, and magnetic stirring was performed at 25°C for 12 h. The mixture was then centrifuged and washed, and dried in a vacuum oven at 60°C for 12 h to obtain polydopamine-coated powder.
[0049] (2) 2.183 g Co(NO3)2·6H2O, 150 mg polydopamine-coated powder and 2.163 g 2-methylimidazole were dissolved in 100 ml, 150 ml and 100 ml methanol, respectively, and named as solution A, solution B and solution C. AB were first mixed and magnetically stirred for 1 h, then solution C was added to the AB mixture, magnetically stirred at room temperature for 12 h, centrifuged and washed 3 to 5 times with methanol centrifugation to obtain the product and dried in a vacuum oven at 80 °C for 12 h to obtain the precursor material.
[0050] (3) The precursor material is heated to 500°C in a high-temperature furnace with nitrogen or argon as protective gas at a heating rate of 5°C / min and calcined for 5 h to obtain the final sample FeCo@C.
[0051] Example 6
[0052] (1) Nickel powder (0.5 μm thick, radial size 10-50 μm) was added at 5 mg / ml into 100 ml of dopamine aqueous solution, wherein the concentration of the dopamine aqueous solution was 1 mg / ml, pH = 8.5, and magnetic stirring was performed at 25°C for 12 h. The powder was then centrifuged and dried in a vacuum oven at 60°C for 12 h to obtain polydopamine-coated powder.
[0053] (2) 1.455 g Co(NO3)2·6H2O, 50 mg polydopamine-coated powder and 1.642 g 2-methylimidazole were dissolved in 100 ml, 150 ml and 100 ml methanol, respectively, and named as solution A, solution B and solution C. AB were first mixed and magnetically stirred for 1 h, then solution C was added to the AB mixture, magnetically stirred at room temperature for 12 h, centrifuged and washed 3 to 5 times with methanol centrifugation to obtain the product and dried in a vacuum oven at 60 ° C for 12 h to obtain the precursor material.
[0054] (3) The precursor material is heated to 900°C in a high-temperature furnace with nitrogen or argon as protective gas at a heating rate of 5°C / min and calcined for 2 h to obtain the final sample NiCo@C.
[0055] Comparative Example 1
[0056] (1) Ball-milled carbonyl iron powder (0.5 μm thick, radial size 10-50 μm) was added at 5 mg / ml into 100 ml of dopamine aqueous solution, wherein the concentration of the dopamine aqueous solution was 1 mg / ml, pH = 8.5, and magnetic stirring was performed at 25°C for 12 h. The mixture was then centrifuged and washed, and dried in a vacuum oven at 60°C for 12 h to obtain polydopamine-coated powder.
[0057] (2) The precursor material is heated to 500°C in a high-temperature furnace with nitrogen or argon as protective gas at a heating rate of 5°C / min and calcined for 5 h to obtain the final sample Fe@C.
[0058] Performance characterization:
[0059] The powders prepared in the above examples and comparative examples were characterized:
[0060] Density: Powder density tester, model: Ruike Instrument FT-100A;
[0061] Wave absorption performance test: vector network analysis tester, model Agilent E8363C PNA microwave network analyzer.
[0062] The characterization results are shown in Table 1:
[0063] Table 1
[0064]
[0065] Note: Filling ratio is the ratio of product powder to paraffin during the wave absorption performance test. The filling ratio and product thickness of the best wave absorption performance of different products are different, while reflection loss and effective absorption bandwidth are the results of wave absorption performance analysis. Generally, metal powder has an optimal filling ratio, and metal powder generally has a filling ratio of 60-70% at most. The filling ratio of iron-based absorbers is generally 60%, which is better.
[0066] The sample thickness in the table is the best matching thickness when the sample has the best microwave absorption performance.
[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a surface-coated modified metal powder material, characterized in that: include: Step S1, coating the surface of metal particles with polydopamine to form polydopamine-coated powder; The metal particles are one or more of carbonyl iron powder, nickel powder, and iron silicon aluminum alloy powder; Step S2, mixing a cobalt source, the polydopamine coated powder, 2-methylimidazole and a solvent, and then reacting to form a reaction slurry; separating the reaction slurry from solid and liquid, and drying to obtain a precursor material; the cobalt source is Co(NO3)2·6H2O; the weight ratio of the cobalt source to the polydopamine coated powder is (1.4-2.2):(0.5-1.5); the weight ratio of the 2-methylimidazole to the cobalt source is (1.6-2.2):(1.4-2.2); Step S3, calcining the precursor material in an inert atmosphere to obtain the surface-coated modified metal powder material.
2. The preparation method according to claim 1, characterized in that: The metal particles are flaky metal powders with a thickness of 0.5 to 2 μm and a radial size of 2 to 100 μm.
3. The preparation method according to claim 1 or 2, characterized in that: The step S1 comprises: mixing the metal particles and the dopamine aqueous solution, and performing an in-situ polymerization reaction under stirring to obtain the polydopamine coated powder.
4. The preparation method according to claim 3, characterized in that: The mass concentration of the dopamine aqueous solution is 1-5 mg / ml.
5. The preparation method according to claim 3, characterized in that: 0.5-5 mg of the metal particles are added to each milliliter of the dopamine aqueous solution.
6. The preparation method according to claim 3, characterized in that: During the in-situ polymerization reaction, the pH value is 7.8-8.
8.
7. The preparation method according to claim 3, characterized in that: The temperature of the in-situ polymerization reaction is 20-40° C. and the time is 12-24 hours.
8. The preparation method according to claim 1, characterized in that: The step S2 comprises: The solvent is divided into at least three parts, the cobalt source is mixed with the first part of the solvent to form a first mixed solution; the polydopamine-coated powder is dispersed in the second part of the solvent to form a second mixed solution; the 2-methylimidazole is mixed with the third part of the solvent to form a third mixed solution; Mixing and stirring the first mixed solution and the second mixed solution to form a pre-reaction solution; The pre-reaction liquid is mixed with the third mixed liquid, and reacted under stirring to form the reaction slurry; After the reaction slurry is centrifugally separated, the precipitate is centrifugally washed and dried to obtain the precursor material.
9. The preparation method according to claim 8, characterized in that: The solvent is an alcohol solvent.
10. The preparation method according to claim 9, characterized in that: The solvent is methanol.
11. The preparation method according to claim 8, characterized in that: After the first mixed liquid and the second mixed liquid are mixed, they are magnetically stirred for 1 to 3 hours to form the pre-reaction liquid; after the pre-reaction liquid and the third mixed liquid are mixed, they are magnetically stirred for 12 to 24 hours at a temperature of 20 to 40° C. to carry out the reaction and obtain the reaction slurry.
12. The preparation method according to claim 1 or 2, characterized in that: In the step S3, during the calcination of the precursor material, the calcination temperature is 500-900° C. and the calcination time is 2-5 hours.
13. A surface-coated modified metal powder material, characterized in that: The method is prepared according to any one of claims 1 to 12.
14. A wave absorbing material, characterized in that: Including the surface-coated modified metal powder material as described in claim 13.