A hexameric or more eutectic high entropy alloy and preparation method thereof
By designing a six-element or more eutectic high-entropy alloy and introducing elements such as Nb, Ta, Mo, and W to form an FCC+Laves structure, the problem of poor strong plasticity matching of existing eutectic high-entropy alloys has been solved and achieved Excellent properties of high yield strength and fracture strain, suitable for industrial production.
Patent Information
- Application Number
- CN202211566409.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-07
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-07
AI Technical Summary
The number of components of existing eutectic high-entropy alloys is mostly less than six elements, making it difficult to give full play to the cocktail effect of high-entropy alloys, and their strong plasticity matching is poor, making it difficult to meet the requirements of industrial production applications.
Design a six-element or more eutectic high-entropy alloy. By selecting Co, Cr, Fe, and Ni as matrix elements, and introducing insoluble metals Nb, Ta, Mo, and W with larger atomic radii, the composition is adjusted to The FCC+Laves structure is formed and prepared using a non-consumable vacuum melting furnace to ensure the high-temperature performance of the alloy.
The alloy has achieved high yield strength and fracture strain, with excellent plastic toughness and mechanical properties. The yield strength is greater than 1200MPa and the fracture strain is greater than 20%, making it suitable for industrial production applications.
Smart Images

Figure CN116240439B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal materials and preparation thereof, and provides a hexameric or more eutectic high entropy alloy and a preparation method thereof. Background Art
[0002] In recent years, high entropy alloys (HEAs) have received extensive attention. The main elements and configuration entropies of such alloys are much higher than those of traditional alloys. As a new material proposed in the 21st century, high entropy alloys have broken through the limitations of traditional alloy elements in the past. High entropy alloys are generally composed of five or more metals or non-metals in an equiatomic ratio or a non-equiatomic ratio. Today, the development of high entropy alloys has also expanded to four or more metals or non-metal elements. Compared with traditional alloys, high entropy alloys have four major effects: high entropy effect, lattice distortion effect, retarded diffusion effect and cocktail effect. These four effects give high entropy alloys many excellent properties, such as high strength and hardness, good wear resistance and corrosion resistance. Among them, the lattice distortion effect makes multi-principal element high entropy alloys have higher hardness and good electrical and thermal conductivity, while the retarded diffusion effect can generally improve the thermal stability of the alloy. In addition, scholars use the cocktail effect to change the composition of the alloy and design some high entropy alloys with extremely superior specific properties.
[0003] Professor Lu Yiping proposed the concept of eutectic high entropy alloy in 2014 and successfully prepared the high strength and high toughness of the cast eutectic high entropy alloy AlCoCrFeNi with both FCC and B2 phases. 2.1 As a new concept in the field of high entropy alloys, eutectic high entropy alloys have shown the world better performance than ordinary alloys. However, the design and preparation of eutectic high entropy alloys have not yet formed a relatively mature system, and still need to be slowly explored and improved in research work.
[0004] Since the concept of eutectic high entropy alloy was proposed, the system of eutectic high entropy alloy has been continuously studied and developed by researchers. As one of the familiar systems, CoCrFeNi high entropy alloy is a single FCC structure. The FCC solid phase has very good plasticity and toughness, but low strength. In order to improve its performance, refractory metals such as Nb, Ta, Mo and W that can produce hard strengthening phase Laves phase are introduced to play the role of solid solution strengthening and second phase strengthening, thereby improving performance. The number of components of current eutectic high entropy alloys is mostly less than six, and more components can further exert the cocktail effect of high entropy alloys. Summary of the invention
[0005] In view of the problem of poor matching between strength and plasticity of existing high entropy alloys, the present invention provides a eutectic high entropy alloy of six elements or more and a preparation method thereof. The high entropy alloy exhibits excellent mechanical properties.
[0006] In order to achieve the purpose of the present invention, the following technical solutions are provided:
[0007] A eutectic high entropy alloy of six or more elements, wherein the raw material components are as follows in terms of atomic molar percentage: Co: 21%-25%, Cr: 21%-25%, Fe: 21%-25%, Ni: 21.75%-22.5%, Nb: 0-14%, Ta: 0-16%, Mo: 0-16%, W: 0-13%, wherein at least two of Nb, Ta, Mo or W are not 0 at the same time.
[0008] In order to avoid harmful impurities in the smelting process that may affect the properties of the alloy, the purity of the metal raw materials is higher than 99.95wt.%
[0009] When Co, Cr, Fe, and Ni are selected as matrix elements and designed with an equiatomic ratio, one of Nb, Ta, Mo, or W is selected as the main element of the eutectic, and one or more other elements are added and their composition is adjusted to obtain a hexameric or more eutectic high entropy alloy.
[0010] The raw material components are as follows in terms of atomic molar percentage: Co: 21.75%, Cr: 21.75%, Fe: 21.75%, Ni: 21.75%, Nb: 8%, Mo: 5%.
[0011] The raw material components are as follows in atomic molar percentage: Co: 22.5%, Cr: 22.5%, Fe: 22.5%, Ni: 22.5%, Nb: 6%, Ta: 4%.
[0012] The raw material components are as follows in terms of atomic molar percentage: Co: 22%, Cr: 22%, Fe: 22%, Ni: 22%, Nb: 5%, Ta: 4%, Mo: 3%.
[0013] The raw material components are as follows in terms of atomic molar percentage: Co: 22%, Cr: 22%, Fe: 22%, Ni: 22%, Nb: 5%, Ta: 3%, Mo: 2%, and W: 2%.
[0014] The method for preparing a hexameric or higher eutectic high entropy alloy is characterized by comprising the following steps:
[0015] (1) Using the eight elements of Co, Cr, Fe, Ni, Nb, Ta, Mo and W as raw materials for batching;
[0016] (2) Remove the surface oxide scale of raw metals Co, Cr, Fe, Ni, Nb, Ta, Mo and W, and clean and dry them;
[0017] (3) Spreading a mixed raw material of Co, Cr, Fe and Ni on the bottom layer of the crucible, placing at least one of Nb, Ta, Mo or W on the upper layer, and then spreading another layer of a mixture of Co, Cr, Fe and Ni on it, and then placing at least one of Nb, Ta, Mo or W, and finally spreading another layer of Co, Cr, Fe and Ni on the top layer; after melting the first layer of CoCrFeNi, shaking the electrode to melt the molten metal and the metal of the second layer, causing a eutectic reaction, and the formed eutectic metal liquid penetrates into the third layer of CoCrFeNi, moving the electrode downward so that the distance between the electrode and the molten metal liquid is maintained at 3-5 mm, and shaking the electrode to melt the metal of the third layer, and so on, to finally obtain a eutectic high entropy alloy of six elements or more.
[0018] In the process, when a non-consumable vacuum melting furnace is used for melting, the vacuum is drawn to 9.5×10 -2 Pa and above, and then filled with argon to -0.5×10 5 Pa and above, further evacuate the furnace with a molecular pump to a pressure of 9.5×10 -3 Pa and above, then fill with argon gas (purity 99.99%) to -0.5×10 5 MPa and above, align the electrode with the crucible filled with pure Ti, and the electrode is 3-5 mm away from the pure Ti, melt for 2-3 min after arcing, then move the arc to the high entropy alloy raw material crucible, set the current intensity to 10-20A, and then slowly increase the current to 50-60A, melt for 30-50s, then increase the current to 120-150A, melt for 1-2 min, increase the current to 280-300A again, melt for 3-4min, finally increase the current to 350A and melt for 1-2 min, repeat this operation 3-6 times to obtain the hexameric or more eutectic high entropy alloy, wherein the alloy is an FCC+Laves structure.
[0019] The order of placing raw materials is from bottom to top, including the following placement methods:
[0020] First, a mixed raw material of Co, Cr, Fe and Ni is placed on the bottom layer of the crucible, and then a mixed raw material of Nb is placed on the upper layer, and then a mixed raw material of Co, Cr, Fe and Ni is placed on it, and then a mixed raw material of Mo is placed, and finally a mixed raw material of Co, Cr, Fe and Ni is placed;
[0021] Alternatively, a mixed raw material of Co, Cr, Fe and Ni is first placed on the bottom layer of the crucible, and then a mixed raw material of Nb is placed on the upper layer, and then a layer of a mixed raw material of Co, Cr, Fe and Ni is placed on it, and then a mixed raw material of Ta is placed, and finally a mixed raw material of Co, Cr, Fe and Ni is placed;
[0022] Alternatively, a mixed raw material of Co, Cr, Fe and Ni is first placed on the bottom layer of the crucible, and then a mixed raw material of Nb and Ta is placed on the upper layer, and then a layer of a mixed raw material of Co, Cr, Fe and Ni is placed on it, and then a mixed raw material of Nb and Mo is placed, and finally a mixed raw material of Co, Cr, Fe and Ni is placed;
[0023] Alternatively, first spread the mixed raw materials of Co, Cr, Fe and Ni on the bottom layer of the crucible, then place the mixed raw materials of Nb and Ta on the upper layer, then spread another layer of the mixed raw materials of Co, Cr, Fe and Ni on it, then put the mixed raw materials of Mo and W, and finally put the mixed raw materials of Co, Cr, Fe and Ni.
[0024] The raw materials are distributed in each layer in equal mass fractions.
[0025] For example, when the raw material components are as follows in atomic molar percentage: Co: 21.75%, Cr: 21.75%, Fe: 21.75%, Ni: 21.75%, Nb: 8%, Mo: 5% alloy, Co: 7.25%, Cr: 7.25%, Fe: 7.25%, Ni: 7.25% are mixed in the bottom layer as the bottom layer, and then Nb: 8% mixture is placed, followed by Co: 7.25%, Cr: 7.25%, Fe: 7.25%, Ni: 7.25% mixture, then Mo: 5% mixture is placed, and then Co: 7.25%, Cr: 7.25%, Fe: 7.25%, Ni: 7.25% mixture is placed.
[0026] The raw material components are as follows in terms of atomic molar percentage: Co: 22.5%, Cr: 22.5%, Fe: 22.5%, Ni: 22.5%, Nb: 6%, Ta: 4%. In the bottom layer, Co: 7.5%, Cr: 7.5%, Fe: 7.5%, Ni: 7.5% are mixed as the bottom layer, and then Nb: 6% mixture is placed, followed by Co: 7.5%, Cr: 7.5%, Fe: 7.5%, Ni: 7.5% mixture, followed by Ta: 4% mixture, and then Co: 7.5%, Cr: 7.5%, Fe: 7.5%, Ni: 7.5% mixture.
[0027] The raw material components are as follows in terms of atomic molar percentage: Co: 22%, Cr: 22%, Fe: 22%, Ni: 22%, Nb: 5%, Ta: 4%, Mo: 3%. In the bottom layer, Co: 7.33%, Cr: 7.3%, Fe: 7.33%, Ni: 7.33% are mixed as the bottom layer, and then Nb: 2.5%, Ta: 4% mixture is placed, and then Co: 7.33%, Cr: 7.33%, Fe: 7.33%, Ni: 7.33% mixture is placed, and then Nb: 2.5%, Mo: 3% mixture is placed, and then Co: 7.33%, Cr: 7.33%, Fe: 7.33%, Ni: 7.33% mixture is placed.
[0028] The raw material components are as follows in terms of atomic molar percentage: Co: 22%, Cr: 22%, Fe: 22%, Ni: 22%, Nb: 5%, Ta: 3%, Mo: 2%, W: 2%. In the bottom layer, Co: 7.33%, Cr: 7.3%, Fe: 7.33%, Ni: 7.33% are mixed as the bottom layer, and then Nb: 5%, Ta: 3% mixture is placed, and then Co: 7.33%, Cr: 7.33%, Fe: 7.33%, Ni: 7.33% mixture is placed, and then W: 2%, Mo: 2% mixture is placed, and then Co: 7.33%, Cr: 7.33%, Fe: 7.33%, Ni: 7.33% mixture is placed.
[0029] The technical concept of the present invention is: the high entropy alloy formed by the atomic ratio of Co, Cr, Fe, Ni, etc. has been reported to be a stable single-phase FCC solid solution, and the alloy with a single-phase FCC structure has good plasticity, but poor strength, and it is difficult to meet the requirements of industrial production and application. In order to improve its performance, by introducing Nb, Ta, Mo and W, which can produce a hard strengthening phase Laves phase, and other insoluble metals with large and similar atomic radii, the effects of solid solution strengthening and second phase strengthening are played to improve the performance. Moreover, Nb, Ta, Mo and W have high melting points, which can make this type of high entropy alloy have good high-temperature performance.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The present invention designs a new type of high entropy alloy through reasonable element selection and composition adjustment, adds Nb, Ta, Mo and W, which are insoluble metals with large atomic radius, into the alloy, effectively adjusts the microstructure and morphology of the alloy, improves the mechanical properties of the alloy, and makes the alloy have good plasticity and high strength and hardness.
[0032] The present invention provides a eutectic high entropy alloy of six elements or more, wherein the high entropy alloy has fine lamellae and uniform structure, the yield strength of the high entropy alloy is greater than or equal to 1200 MPa, the fracture strain is greater than or equal to 20%, and the high strength and excellent plasticity and toughness are exhibited. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is the XRD spectrum of the cast state of the eutectic high entropy alloy with six or more elements.
[0034] Figure 2 This is the room temperature compressive engineering stress-strain curve of the cast eutectic high entropy alloy with six or more elements.
[0035] Figure 3 The metallographic phase diagram of the cast state of the eutectic high entropy alloy with six or more elements, wherein (A) is (CoCrFeNi) 90 Nb6Ta4; (B) is (CoCrFeNi) 87 Nb8Mo5; (C) is (CoCrFeNi) 88 Nb5Ta4Mo3;
[0036] (D) is (CoCrFeNi) 88 Nb5Ta4Mo3W2.
[0037] Figure 4 This is the DTA differential thermal analysis of the cast state of eutectic high entropy alloy with six or more elements. DETAILED DESCRIPTION
[0038] The microstructure characterization and mechanical property test information of the high entropy alloy are as follows:
[0039] (1) Phase analysis: X-ray diffraction analysis was performed using an Ultima IV Cu Kα diffractometer (λ = 1.54 Å) with an operating voltage and current of 40 kV and 40 mA, respectively, with a 2θ scanning range from 20° to 100° and a speed of 4°C / min.
[0040] (2) Mechanical properties: According to the relevant requirements of GB / T 7314-2017 Metal Material Room Temperature Compression Test Method, a room temperature compression test was carried out, and the experimental compression loading rate was 0.36 mm / min. Two experiments were carried out for each component alloy, and the stress-strain curve data was the average of the two experiments.
[0041] (3) Microstructure: The sample structure was observed under different magnifications using a scanning electron microscope.
[0042] (4) Differential thermal analysis: By measuring the phase change and thermal effect of the metal, when a eutectic reaction occurs, only one phase change will occur, producing an exothermic (endothermic) peak.
[0043] The present invention will be further described below in conjunction with specific embodiments and comparative examples.
[0044] Example 1
[0045] A eutectic high entropy alloy (CoCrFeNi) containing six or more elements 90 Nb6Ta4, in which the atomic percentages of elements are Co: 22.5%, Cr: 22.5%, Fe: 22.5%, Ni: 22.5%, Nb: 6%, and Ta: 4%.
[0046] Step 1: Select metal particles of six elements, namely Co, Cr, Fe, Ni, Nb and Ta, as raw materials, and the purity of all metal raw materials is greater than 99.95wt.%.
[0047] Step 2: The molar ratio of Co:Cr:Fe:Ni:Nb:Ta of the alloy is 22.5%:22.5%:22.5%:22.5%:6%:4%, and the mass percentage is converted according to the molar percentage of the multi-component refractory eutectic alloy. Based on the total mass of each alloy ingot being 40g, each single element raw material is weighed using an electronic balance. The weighed masses of the single element raw materials Co, Cr, Fe, Ni, Nb and Ta are 8.347g, 7.365g, 7.910g, 8.313g, 3.509g and 4.556g, respectively, with a weighing error of ±0.001g.
[0048] Step 3: Use different types (240#, 400# and 800#) of SiC sandpaper to polish the surfaces of the metal raw materials Co, Cr, Fe, Ni, Nb and Ta (purity is 99.95wt.%) to remove the oxide scale and impurities on the surface, and clean them with anhydrous ethanol. After fully drying, put them into sealed bags for standby use.
[0049] Step 4. According to the melting point of the alloy, place Co, Cr, Fe and Ni on the bottom layer of the crucible, Ta (Mo) on the upper layer, and then place another layer of Co, Cr, Fe and Ni on it, and then place Nb (W), and finally place another layer of Co, Cr, Fe and Ni on the top layer. The top layer of Co, Cr, Fe and Ni should be placed at 1 / 3 of the total amount, and then Nb should be added. The second layer should still contain 1 / 3 of the total amount of Co, Cr, Fe and Ni, and then Ta should be added. Finally, 1 / 3 of Co, Cr, Fe and Ni should be placed on the bottom layer. This arrangement ensures that Co, Cr, Fe and Ni have sufficient eutectic reaction with the refractory metal Nb, so that the formed molten metal has a lower melting point and good fluidity. The first vacuum to 9.5×10 -1 Pa, high-purity argon gas (purity 99.99%) was filled to -0.5×105 MPa, and then the second vacuuming was performed, and the pressure in the furnace was evacuated to 9.5×10 -3 Pa, and then filled with argon to -0.5×10 5 MPa, align the electrode tungsten rod with the middle of the crucible filled with pure Ti, keep the distance between the tungsten rod and the pure Ti about 3-5mm, and melt for 1-2min after arcing. Then move the electrode tungsten rod to align with the high entropy alloy raw material sample to be melted, control the current to about 20A and then strike the arc, then slowly increase the current to 60A, melt for 35s, then increase the current to 130A, melt for 1.5 min, increase the current to 300A again, melt for 3.5min, and finally increase the current to 350A and melt for 2 min. After each melting, after the alloy cools, use a manipulator to turn the alloy ingot over and remelt it, repeat this operation 6 times to obtain the refractory eutectic high entropy alloy.
[0050] For (CoCrFeNi) in the embodiment 90 The phase analysis of Nb6Ta4 high entropy alloy sample shows the X-ray diffraction (XRD) spectrum as shown below: Figure 1 As shown. It can be seen from the figure (CoCrFeNi) 90 Nb6Ta4 alloy has FCC+Laves structure.
[0051] For (CoCrFeNi) in the embodiment 90 The microstructure of the Nb6Ta4 high entropy alloy sample was analyzed, and the scanning electron microscope (SEM) photos are shown in Figure 3 (A), from the figure analysis, (CoCrFeNi) 90 Nb6Ta4 alloy is a uniform lamellar structure, and the grain boundaries are irregular eutectics caused by element enrichment and latent heat of crystallization. The structure is formed by alternating FCC phase and Laves phase.
[0052] For (CoCrFeNi) in the embodiment 90 The Nb6Ta4 high entropy alloy sample was subjected to room temperature compression test, and its compression true stress-strain curve is shown in Figure 2 As shown, it can be seen that (CoCrFeNi) 90 The yield strength of Nb6Ta4 alloy is 1175.3MPa, the compressive strength is 2401MPa, and the fracture strain is 30%. It has high strength and exhibits good plasticity and toughness.
[0053] For this example (CoCrFeNi) 90 Nb6Ta4 high entropy alloy samples were subjected to differential thermal analysis, such as Figure 4 As shown, the high entropy alloy has only one endothermic peak, which is a eutectic reaction.
[0054] Example 2
[0055] This embodiment discloses a eutectic high entropy alloy of six or more elements, the general formula of which is (CoCrFeNi) 87 Nb8Mo5. The atomic percentages of the elements are Co: 21.75%, Cr: 21.75%, Fe: 21.75%, Ni: 21.75%, Nb: 8%, Mo: 5%. The top layer of Co, Cr, Fe and Ni should be placed at 1 / 3 of the total, followed by Nb, the second layer still has Co, Cr, Fe and Ni at 1 / 3 of the total, then Mo is added, and the last 1 / 3 of Co, Cr, Fe and Ni is placed at the bottom layer.
[0056] The preparation method of the hexameric or higher eutectic high entropy alloy in this embodiment is the same as that in Example 1.
[0057] For (CoCrFeNi) in the embodiment 87 The phase analysis of Nb8Mo5 high entropy alloy sample is shown in the X-ray diffraction (XRD) spectrum. Figure 1 As shown. It can be seen from the figure (CoCrFeNi) 87 Nb8Mo5 alloy has a FCC+Laves phase structure.
[0058] For this example (CoCrFeNi) 87 The microstructure of Nb8Mo5 high entropy alloy samples was analyzed, and the scanning electron microscope (SEM) photos are shown in Figure 3 (B), from the analysis of the figure, (CoCrFeNi) 87 Nb8Mo5 alloy is a uniform lamellar structure, and the grain boundaries are irregular eutectics caused by element enrichment and latent heat of crystallization. The structure is formed by alternating FCC phases and Laves phases.
[0059] For this example (CoCrFeNi) 87 The compression true stress-strain curve of Nb8Mo5 high entropy alloy sample was tested at room temperature. Figure 2 As shown, it can be seen that (CoCrFeNi) 87 The yield strength of Nb8Mo5 alloy is 1321MPa, the compressive strength is 2294MPa, and the fracture strain is 22%. It has high strength and exhibits good plasticity and toughness.
[0060] For this example (CoCrFeNi) 87 Differential thermal analysis of Nb8Mo5 high entropy alloy samples, such as Figure 4 As shown, the high entropy alloy has only one endothermic peak, which is a eutectic reaction.
[0061] Example 3
[0062] This embodiment discloses a eutectic high entropy alloy of six or more elements, the general formula of which is (CoCrFeNi) 88 The atomic percentages of elements in Nb5Ta4Mo3 are Co: 22%, Cr: 22%, Fe: 22%, Ni: 22%, Nb: 5%, Ta: 4%, and Mo: 3%.
[0063] The top layer of Co, Cr, Fe and Ni should account for 1 / 3 of the total, followed by 1 / 2 of Nb and Ta. The second layer still contains 1 / 3 of Co, Cr, Fe and Ni, followed by 1 / 2 of Nb and Mo. Finally, 1 / 3 of Co, Cr, Fe and Ni are placed on the bottom layer.
[0064] The preparation method of the hexameric or higher eutectic high entropy alloy in this embodiment is the same as that in Example 1.
[0065] For (CoCrFeNi) in the embodiment 88 Nb5Ta4Mo3, high entropy alloy sample was subjected to phase analysis, and its X-ray diffraction (XRD) spectrum is shown as follows Figure 1 As shown. It can be seen from the figure (CoCrFeNi) 88 Nb5Ta4Mo3, the alloy has FCC+Laves phase structure.
[0066] For this example (CoCrFeNi) 88 Nb5Ta4Mo3, high entropy alloy samples were subjected to microstructural analysis, and scanning electron microscope (SEM) photos were shown in Figure 3 (C), from the figure analysis, (CoCrFeNi) 88 Nb5Ta4Mo3, the alloy is a uniform lamellar structure, and the grain boundaries are irregular eutectics caused by element enrichment and latent heat of crystallization. The structure is formed by alternating FCC phases and Laves phases.
[0067] For this example (CoCrFeNi) 88 Nb5Ta4Mo3, high entropy alloy sample was subjected to room temperature compression test, and its compression true stress-strain curve is as follows Figure 2 As shown, it can be seen that (CoCrFeNi) 88 Nb5Ta4Mo3, the alloy has a yield strength of 1324MPa, a compressive strength of 2252MPa, and a fracture strain of 20.1%. It has high strength and exhibits good plasticity and toughness.
[0068] For this example (CoCrFeNi) 88 Differential thermal analysis of Nb5Ta4Mo3 high entropy alloy samples, such as Figure 4As shown, the high entropy alloy has only one endothermic peak, which is a eutectic reaction.
[0069] Example 4
[0070] This embodiment discloses a eutectic high entropy alloy of six or more elements, the general formula of which is (CoCrFeNi) 88 Nb5Ta3Mo2W2, in which the atomic percentages of elements are Co: 22%, Cr: 22%, Fe: 22%, Ni: 22%, Nb: 5%, Ta: 3%, Mo: 2%, and W: 2%.
[0071] The top layer of Co, Cr, Fe and Ni should account for 1 / 3 of the total, followed by Nb and Mo. The second layer still contains Co, Cr, Fe and Ni at 1 / 3 of the total, followed by Mo and W. The last 1 / 3 of Co, Cr, Fe and Ni are placed on the bottom layer.
[0072] The preparation method of the hexameric or higher eutectic high entropy alloy in this embodiment is the same as that in Example 1.
[0073] For (CoCrFeNi) in the embodiment 88 The phase analysis of Nb5Ta3Mo2W2 high entropy alloy sample is shown in the X-ray diffraction (XRD) spectrum. Figure 1 As shown. It can be seen from the figure (CoCrFeNi) 88 Nb5Ta3Mo2W2 alloy has FCC+Laves phase structure.
[0074] For this example (CoCrFeNi) 88 The microstructure of the Nb5Ta3Mo2W2 high entropy alloy sample was analyzed, and the scanning electron microscope (SEM) photos are shown in Figure 3 (D), from the analysis of the figure, (CoCrFeNi) 88 Nb5Ta3Mo2W2 alloy is a uniform lamellar structure, and the grain boundaries are irregular eutectics caused by element enrichment and latent heat of crystallization. The structure is formed by alternating FCC phases and Laves phases.
[0075] For this example (CoCrFeNi) 88 The compression true stress-strain curve of Nb5Ta3Mo2W2 high entropy alloy sample was subjected to room temperature compression test. Figure 2 As shown, it can be seen that (CoCrFeNi) 88 The yield strength of Nb5Ta3Mo2W2 alloy is 1281MPa, the compressive strength is 2424MPa, and the fracture strain is 29%. It has high strength and exhibits good plasticity and toughness.
[0076] For this example (CoCrFeNi) 88 Differential thermal analysis of Nb5Ta3Mo2W2 high entropy alloy samples, such as Figure 4 As shown, the high entropy alloy has only one endothermic peak, which is a eutectic reaction.
[0077] Comparative Example 1
[0078] A eutectic high entropy alloy (CoCrFeNi) containing six or more elements 88 Nb5Ta3Mo2W2, in which the atomic percentages of elements are Co: 22%, Cr: 22%, Fe: 22%, Ni: 22%, Nb: 5%, Ta: 3%, Mo: 2%, and W: 2%.
[0079] For the eutectic high entropy alloy (CoCrFeNi) in this case 88 The layered arrangement of Nb5Ta3Mo2W2 is to place Co, Cr, Fe and Ni in the upper layer, Nb, Ta and Mo in the middle layer, and W in the bottom layer. When smelting is performed in the manner of Example 1, Nb, Ta, Mo and W with the highest melting points melt unevenly, some form eutectic, some form hypereutectic and hypoeutectic, and the structure is extremely uneven. Even W with the highest melting point in the final structure still exists in the form of a single substance, affecting the alloy properties.
[0080] The above content is a further detailed description of the present invention in combination with specific implementation methods, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, several simple deductions or substitutions can be made. All high entropy alloys in which Nb, Ta, Mo and W are infinitely dissolved in the CoCrFeNi-(NbTaMoW) series high entropy alloys described in the present invention and produce eutectic reactions with CoCrFeNi should be regarded as belonging to the protection scope of the present invention.
Claims
1. A 6-element or more eutectic high entropy alloy, characterized in that: The raw material components are as follows in terms of atomic molar percentage: Co: 21%~25%, Cr: 21%~25%, Fe: 21%~25%, Ni: 21.75%~22.5%, Nb: 0~14%, Ta: 0~16%, Mo: 0~16%, W: 0~13%, wherein at least two of Nb, Ta, Mo or W are not 0; The hexameric or higher eutectic high entropy alloy has an FCC+Laves structure; and the structure is formed by alternating arrangement of the formed FCC phase and Laves phase.
2. The hexameric or more eutectic high entropy alloy according to claim 1, characterized in that: When Co, Cr, Fe, and Ni are selected as matrix elements and designed with an equiatomic ratio, one of Nb, Ta, Mo, or W is selected as the main element of the eutectic, and one or more other elements are added and their composition is adjusted to obtain a hexameric or more eutectic high entropy alloy.
3. The hexameric or more eutectic high entropy alloy according to claim 2, characterized in that: The raw material components are as follows in atomic mole percentage: Co: 21.75%, Cr: 21.75%, Fe: 21.75%, Ni: 21.75%, Nb: 8%, Mo: 5%.
4. The hexameric or more eutectic high entropy alloy according to claim 2, characterized in that: The raw material components are as follows in atomic mole percentage: Co: 22.5%, Cr: 22.5%, Fe: 22.5%, Ni: 22.5%, Nb: 6%, Ta: 4%.
5. The hexameric or more eutectic high entropy alloy according to claim 2, characterized in that: The raw material components are as follows in atomic mole percentage: Co: 22%, Cr: 22%, Fe: 22%, Ni: 22%, Nb: 5%, Ta: 4%, Mo: 3%.
6. The hexameric or more eutectic high entropy alloy according to claim 2, characterized in that: The raw material components are as follows in atomic mole percentage: Co: 22%, Cr: 22%, Fe: 22%, Ni: 22%, Nb: 5%, Ta: 3%, Mo: 2%, W: 2%.
7. The method for preparing a hexameric or more eutectic high entropy alloy according to any one of claims 1 to 6, characterized in that: The steps include: (1) Using eight elements of Co, Cr, Fe, Ni, Nb, Ta, Mo and W as described in any one of claims 1 to 6 as raw materials for batching; (2) Remove the surface oxide scale of raw metals Co, Cr, Fe, Ni, Nb, Ta, Mo and W, and clean and dry them; (3) Spreading a mixed raw material of Co, Cr, Fe and Ni on the bottom layer of the crucible, placing at least one of Nb, Ta, Mo or W on the upper layer, and then spreading another layer of a mixture of Co, Cr, Fe and Ni on it, and then placing at least one of Nb, Ta, Mo or W, and finally spreading another layer of Co, Cr, Fe and Ni on the top layer; after melting the first layer of CoCrFeNi, shaking the electrode to melt the molten metal and the metal of the second layer, causing a eutectic reaction, and the formed eutectic metal liquid penetrates into the third layer of CoCrFeNi, moving the electrode downward so that the distance between the electrode and the molten metal liquid is maintained at 3-5 mm, and shaking the electrode to melt the metal of the third layer, and so on, to finally obtain a eutectic high entropy alloy of six elements or more.
8. The method for preparing a 6-element or more eutectic high entropy alloy according to claim 7, characterized in that: When using a non-consumable vacuum melting furnace for melting, the vacuum is pumped to 9.5×10 -2 Pa and above, and then filled with argon to -0.5×10 5 Pa and above, further evacuate the furnace with a molecular pump to a pressure of 9.5×10 -3 Pa and above, then fill with argon to -0.5×10 5 MPa and above, align the electrode with the crucible filled with pure Ti, and the electrode is 3-5mm away from the pure Ti, melt for 2-3 min after arcing, then move the arc to the high entropy alloy raw material crucible, set the current intensity to 10-20A, and then slowly increase the current to 50-60A, melt for 30-50s, then increase the current to 120-150A, melt for 1-2 min, increase the current to 280-300A again, melt for 3-4min, finally increase the current to 350A and melt for 1-2 min, repeat this operation 3-6 times to obtain the hexameric or more eutectic high entropy alloy, the alloy is an FCC+Laves structure.
9. The method for preparing a hexameric or higher eutectic high entropy alloy according to claim 8, characterized in that: The order of placing raw materials is from bottom to top, including the following placement methods: First, a mixed raw material of Co, Cr, Fe and Ni is placed on the bottom layer of the crucible, and then a mixed raw material of Nb and Mo is placed on the upper layer, and then a mixed raw material of Co, Cr, Fe and Ni is placed on it, and then a mixed raw material of Nb and Mo is placed, and finally a mixed raw material of Co, Cr, Fe and Ni is placed; Alternatively, a mixed raw material of Co, Cr, Fe and Ni is first placed on the bottom layer of the crucible, and then a mixed raw material of Nb and Ta is placed on the upper layer, and then a layer of a mixed raw material of Co, Cr, Fe and Ni is placed on top, and then a mixed raw material of Nb and Ta is placed, and finally a mixed raw material of Co, Cr, Fe and Ni is placed; Alternatively, a mixed raw material of Co, Cr, Fe and Ni is first placed on the bottom layer of the crucible, and then a mixed raw material of Nb and Ta is placed on the upper layer, and then a layer of a mixed raw material of Co, Cr, Fe and Ni is placed on it, and then a mixed raw material of Nb and Mo is placed, and finally a mixed raw material of Co, Cr, Fe and Ni is placed; Alternatively, first spread the mixed raw materials of Co, Cr, Fe and Ni on the bottom layer of the crucible, then place the mixed raw materials of Nb and Ta on the upper layer, then spread another layer of the mixed raw materials of Co, Cr, Fe and Ni on it, then put the mixed raw materials of Mo and W, and finally put the mixed raw materials of Co, Cr, Fe and Ni.
10. The method for preparing a hexameric or higher eutectic high entropy alloy according to claim 9, characterized in that: The raw materials are distributed in each layer in equal mass fractions.
Citation Information
Patent Citations
High-temperature alloy with low content of cobalt and nickel
CN101130844A