A negative electrode slurry, its preparation method and application

The preparation of negative electrode slurry by aqueous ultraviolet curing technology solves the problem of long production cycle of lithium-ion battery negative electrode materials, realizes rapid curing and environmentally friendly high-efficiency production, enhances the adhesion between the electrode sheet and the substrate, and improves the stability of the battery.

CN116247177BActive Publication Date: 2026-11-10SHENZHEN HAODYNE TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310051426.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-02
Publication Date
2026-11-10
Estimated Expiration
2043-02-02

AI Technical Summary

Technical Problem

The production cycle of existing lithium-ion battery anode materials is long, especially the electrode drying time is too long, which affects production efficiency, and traditional curing technology may cause environmental damage.

Method used

A negative electrode slurry was prepared using water-based ultraviolet light curing technology. Water-soluble materials and deionized water were used as dispersion media, and rapid cross-linking and curing were achieved through ultraviolet light curing technology to prepare the negative electrode material.

Benefits of technology

It shortens the electrode production time, improves production efficiency, enhances the adhesion between the negative electrode material and the substrate, and maintains the stability and environmental friendliness of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004058189360000021
    Figure BDA0004058189360000021
  • Figure BDA0004058189360000031
    Figure BDA0004058189360000031
  • Figure BDA0004058189360000041
    Figure BDA0004058189360000041
Patent Text Reader

Abstract

This invention provides a negative electrode slurry, its preparation method, and its application. The negative electrode slurry comprises, by weight, the following components: 80-95 parts of active material, 1-5 parts of conductive agent, 1-5 parts of water-based photocurable polymer material, 1-4 parts of water-based photocurable small molecule material, 0.1-3 parts of water-based photoinitiator, and 20-100 parts of deionized water. This invention provides a negative electrode slurry that can significantly improve battery production efficiency, enhance the adhesion between the negative electrode material and the substrate, and exhibit good performance under high and low temperature environments. This invention also provides a method for preparing negative electrode materials using water-based photocuring technology, which has the advantage of being environmentally friendly and does not produce gases with a noticeable pungent odor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of negative electrode material technology, specifically relating to a negative electrode slurry, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries have attracted widespread attention due to their advantages such as high output power, high energy density, and no memory effect, and are therefore widely used in digital and 3C electronic products and power batteries. The structure of a lithium-ion battery mainly consists of a positive electrode, a negative electrode, a separator, an electrolyte, and a casing. Existing technologies disclose the production of negative electrode sheets by preparing the negative electrode material into a paste using a binder, then coating it onto the surface of a metal foil, followed by drying, rolling, and cutting processes. This production method has a long production cycle, especially the drying time of the electrode sheets, which can reach more than ten hours, becoming a major factor limiting battery production efficiency. Therefore, shortening the drying time of the electrode sheets will help improve the overall battery production efficiency.

[0003] In recent years, ultraviolet (UV) curing technology has emerged as an environmentally friendly green technology, with its greatest advantages being short curing time and excellent product performance. The basic principle of UV free radical curing is that under UV light irradiation, the photoinitiator in the curing system absorbs photons to generate free radicals, thereby initiating the instantaneous polymerization of unsaturated double bonds in the system, ultimately forming a photocured linear or network structure. This curing technology is characterized by high efficiency, environmental friendliness, energy saving, economy, and high quality. With its rapid development over the past few decades, UV curing technology has been widely applied in coatings, inks, plastics, adhesives, and electronics.

[0004] UV curing technology offers significant advantages over traditional curing techniques; however, it still suffers from some drawbacks, such as the need to add diluents and organic solvents in certain systems. These reactive diluents often have adverse effects on human health and the environment. Therefore, water-based UV curing technology has become a crucial solution to these problems.

[0005] Waterborne photopolymerization technology not only possesses the advantages of photopolymerization technology, but also uses water as a dispersant, avoiding the use of organic solvents and diluents. During the preparation process, the evaporation of water does not impact the environment. Currently, most battery anode materials are also water-based systems, indicating significant potential for the application of photopolymerization technology in the preparation of anode materials.

[0006] Therefore, there is an urgent need in this field to develop a method for preparing anode materials using aqueous photocuring technology that not only does not harm the environment, but also produces lithium-ion batteries with good electrochemical performance. Summary of the Invention

[0007] To address the shortcomings of existing technologies, the present invention aims to provide a negative electrode slurry, its preparation method, and its applications. The present invention provides a negative electrode slurry that can significantly improve battery production efficiency, enhance the adhesion between the negative electrode material and the substrate, and exhibit good performance under high and low temperature environments. The present invention also provides a method for preparing negative electrode materials using water-based photopolymerization technology, which has the advantage of being environmentally friendly and does not produce gases with a noticeable pungent odor.

[0008] To achieve this objective, the present invention adopts the following technical solution:

[0009] In a first aspect, the present invention provides a negative electrode slurry, the negative electrode slurry comprising the following components by weight:

[0010]

[0011] On the one hand, the negative electrode slurry provided by this invention does not require the use of organic solvents in the slurry preparation process. All its components are water-soluble materials, and deionized water is used as the dispersion medium, resulting in no significant pungent gas volatilization and making it environmentally friendly. On the other hand, the negative electrode slurry provided by this invention uses ultraviolet light curing technology, which enables rapid cross-linking and curing, thus improving production efficiency.

[0012] Furthermore, by controlling the content of the above-mentioned components, the present invention can not only ensure the normal progress of the preparation process, but also effectively prevent the powder from settling in the slurry, thus achieving better slurry uniformity.

[0013] In this invention, the active material is 80-95 parts by weight, for example, 80 parts, 82 parts, 85 parts, 88 parts, 90 parts, 92 parts, 95 parts, etc.

[0014] In this invention, the conductive agent is 1-5 parts by weight, for example, 1 part, 2 parts, 3 parts, 4 parts, 5 parts, etc.

[0015] In this invention, the water-based photocurable polymer material is 1-5 parts by weight, for example, 1 part, 2 parts, 3 parts, 4 parts, 5 parts, etc.

[0016] In this invention, the water-based photocurable small molecule material is 1-4 parts by weight, for example, 1 part, 2 parts, 3 parts, 4 parts, etc.

[0017] In this invention, the aqueous photoinitiator is 0.1-3 parts by weight, for example, 0.1 parts, 0.2 parts, 0.5 parts, 0.8 parts, 1 part, 2 parts, 3 parts, etc.

[0018] In this invention, the deionized water is in the range of 20-100 parts by weight, for example, 20 parts, 30 parts, 40 parts, 50 parts, 60 parts, 70 parts, 80 parts, 90 parts, 100 parts, etc.

[0019] Preferably, the negative electrode slurry comprises the following components by weight:

[0020]

[0021]

[0022] Preferably, the active material includes any one or a combination of at least two of lithium titanate, titanium dioxide, graphite, mesophase carbon microspheres, elemental silicon, silicon oxides, or silicon alloys.

[0023] Preferably, the average particle size of the active material is 5-20 μm, more preferably 8-18 μm, for example, it can be 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, etc.

[0024] Preferably, the conductive agent includes any one or a combination of at least two of carbon nanotubes, conductive carbon black, or graphene.

[0025] Preferably, the waterborne photocurable polymer material includes waterborne unsaturated polyester resin and / or waterborne unsaturated acrylate resin.

[0026] In this invention, the addition of the above-mentioned water-based photocurable polymer materials has the advantages of improving the overall flexibility of the electrode and maintaining good processing performance.

[0027] Preferably, the molecular weight of the waterborne unsaturated polyester resin is 10,000 to 1,000,000, more preferably 50,000 to 800,000, and can be, for example, 10,000, 20,000, 50,000, 80,000, 100,000, 200,000, 400,000, 600,000, 800,000, 1,000,000, etc.

[0028] In this invention, by adjusting the molecular weight of the water-based unsaturated polyester resin, the mechanical properties of the cured electrode are good. If the molecular weight is too low, the electrode will have poor water resistance and decreased mechanical properties. Conversely, if the molecular weight is too high, the viscosity of the slurry will be too high, which will affect the processing performance.

[0029] Preferably, the waterborne unsaturated acrylate resin includes any one or a combination of at least two of the following: waterborne epoxy-modified unsaturated acrylate resin, waterborne polyether-modified unsaturated acrylate resin, waterborne silicone-modified unsaturated acrylate resin, or waterborne polyurethane-modified unsaturated acrylate resin.

[0030] Preferably, the waterborne photocurable small molecule material includes any one or a combination of at least two of the following: (meth)acrylate-2-hydroxyethyl acrylate, (meth)acrylate-hydroxypropyl acrylate, ethoxyethoxyethyl acrylate, methoxy polyethylene glycol (meth)acrylate, dipropylene glycol diacrylate, triethylene glycol di(meth)acrylate, polyethylene glycol (e.g., polyethylene glycol 200, polyethylene glycol 300 or polyethylene glycol 400) diacrylate, polypropylene glycol (e.g., polypropylene glycol 400) diacrylate, tetraethylene glycol dimethacrylate, or polyethylene glycol (e.g., polyethylene glycol 200 or polyethylene glycol 400) dimethacrylate.

[0031] Preferably, the aqueous photoinitiator is any one or a combination of at least two of the following: aqueous benzoin derivatives, aqueous acetophenone derivatives, or aqueous organophosphorus compounds.

[0032] In a second aspect, the present invention provides a method for preparing the negative electrode slurry according to the first aspect, the method comprising the following steps:

[0033] (1) The active material, conductive agent, water-based photocurable small molecule material and water-based photoinitiator are mixed once to obtain the first mixture;

[0034] (2) The first mixture obtained in step (1) is mixed with the water-based photocurable polymer material a second time to obtain the second mixture. Then the second mixture is mixed with deionized water a third time and filtered to obtain the negative electrode slurry.

[0035] Preferably, the mixing in step (1) is carried out under stirring.

[0036] Preferably, the secondary and tertiary mixing in step (2) are both carried out under stirring.

[0037] Thirdly, the present invention provides a negative electrode sheet, which is prepared from the negative electrode slurry according to the first aspect.

[0038] In this invention, the method for preparing the above-mentioned negative electrode sheet includes the following steps:

[0039] The negative electrode slurry is coated onto the surface of copper foil using a coating machine. The built-in drying system briefly heats and dries the electrode, followed by ultraviolet light curing to obtain the negative electrode.

[0040] In this invention, the negative electrode sheet is first prepared using ultraviolet light curing technology, which has the advantages of saving electrode sheet production time and improving work efficiency. Secondly, due to the chemical bonding that occurs during the curing process, the adhesion between the binder and the powder, and between the electrode sheet and the foil, is enhanced, thereby effectively maintaining the stability of the battery.

[0041] Fourthly, the present invention provides a lithium-ion battery, the lithium-ion battery comprising a positive electrode, a negative electrode, an electrolyte and a separator, wherein the negative electrode is the negative electrode according to the third aspect.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] This invention provides a negative electrode slurry that does not require the use of organic solvents in the slurry preparation process. All components used are water-soluble materials, and deionized water is used as the dispersion medium. There is no obvious pungent gas volatilization, making it environmentally friendly.

[0044] This invention employs ultraviolet light curing technology to prepare negative electrode sheets, which has the advantages of saving electrode sheet production time and improving work efficiency. Secondly, due to the chemical bonding that occurs during the curing process, the adhesion between the binder and the powder, and between the electrode sheet and the foil material, is enhanced, thereby effectively maintaining the stability of the battery. Detailed Implementation

[0045] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0046] Example 1

[0047] This embodiment provides a negative electrode slurry, which comprises the following components by weight: 90 parts graphite (average particle size of 13 μm), 3 parts conductive carbon black, 3 parts waterborne polyester modified unsaturated acrylate resin (model KDD704, purchased from Keding Company), 2 parts (meth)acrylate-2-hydroxyethyl ester, 1.5 parts α,α-diethoxyacetophenone, and 60 parts deionized water.

[0048] This embodiment provides a method for preparing the above-mentioned negative electrode slurry, which includes the following steps:

[0049] (1) The above-mentioned active material, conductive agent, water-based photocurable small molecule material and water-based photoinitiator are stirred to obtain a first mixture;

[0050] (2) Stir the first mixture obtained in step (1) and the water-based photocurable polymer material to obtain the second mixture. Then stir the second mixture and deionized water, filter and obtain the negative electrode slurry.

[0051] This embodiment also provides a negative electrode sheet and its preparation method, the preparation method is as follows:

[0052] The negative electrode slurry is coated onto the surface of copper foil using a coating machine. The built-in drying system briefly heats and dries the electrode, followed by ultraviolet light curing to obtain the negative electrode.

[0053] Example 2

[0054] This embodiment provides a negative electrode slurry, which comprises the following components by weight: 85 parts graphite (average particle size of 10 μm), 1 part conductive carbon black, 1 part waterborne polyester modified unsaturated acrylate resin (model KDD704, purchased from Keding Company), 1 part (meth)acrylate-2-hydroxyethyl ester, 0.1 part α,α-diethoxyacetophenone, and 50 parts deionized water.

[0055] This embodiment provides a method for preparing the above-mentioned negative electrode slurry, which includes the following steps:

[0056] (1) The above-mentioned active material, conductive agent, water-based photocurable small molecule material and water-based photoinitiator are stirred to obtain a first mixture;

[0057] (2) Stir the first mixture obtained in step (1) and the water-based photocurable polymer material to obtain the second mixture. Then stir the second mixture and deionized water, filter and obtain the negative electrode slurry.

[0058] This embodiment also provides a negative electrode sheet and its preparation method, the preparation method is as follows:

[0059] The negative electrode slurry is coated onto the surface of copper foil using a coating machine. The built-in drying system briefly heats and dries the electrode, followed by ultraviolet light curing to obtain the negative electrode.

[0060] Example 3

[0061] This embodiment provides a negative electrode slurry, which comprises the following components by weight: 92 parts graphite (average particle size of 11 μm), 5 parts conductive carbon black, 3 parts waterborne polyester modified unsaturated acrylate resin (model KDD704, purchased from Keding Company), 2 parts (meth)acrylate-2-hydroxyethyl ester, 2 parts α,α-diethoxyacetophenone, and 100 parts deionized water.

[0062] This embodiment provides a method for preparing the above-mentioned negative electrode slurry, which includes the following steps:

[0063] (1) The above-mentioned active material, conductive agent, water-based photocurable small molecule material and water-based photoinitiator are stirred to obtain a first mixture;

[0064] (2) Stir the first mixture obtained in step (1) and the water-based photocurable polymer material to obtain the second mixture. Then stir the second mixture and deionized water, filter and obtain the negative electrode slurry.

[0065] This embodiment also provides a negative electrode sheet and its preparation method, the preparation method is as follows:

[0066] The negative electrode slurry is coated onto the surface of copper foil using a coating machine. The built-in drying system briefly heats and dries the electrode, followed by ultraviolet light curing to obtain the negative electrode.

[0067] Example 4

[0068] This embodiment provides a negative electrode slurry, which comprises the following components by weight: 80 parts graphite (average particle size of 5 μm), 1 part conductive carbon black, 1 part waterborne polyester modified unsaturated acrylate resin (model KDD704, purchased from Keding Company), 1 part (meth)acrylate-2-hydroxyethyl ester, 0.1 part α,α-diethoxyacetophenone, and 20 parts deionized water.

[0069] This embodiment provides a method for preparing the above-mentioned negative electrode slurry, which includes the following steps:

[0070] (1) The above-mentioned active material, conductive agent, water-based photocurable small molecule material and water-based photoinitiator are stirred to obtain a first mixture;

[0071] (2) Stir the first mixture obtained in step (1) and the water-based photocurable polymer material to obtain the second mixture. Then stir the second mixture and deionized water, filter and obtain the negative electrode slurry.

[0072] This embodiment also provides a negative electrode sheet and its preparation method, the preparation method is as follows:

[0073] The negative electrode slurry is coated onto the surface of copper foil using a coating machine. The built-in drying system briefly heats and dries the electrode, followed by ultraviolet light curing to obtain the negative electrode.

[0074] Example 5

[0075] This embodiment provides a negative electrode slurry, which comprises the following components by weight: 95 parts graphite (average particle size of 20 μm), 5 parts conductive carbon black, 5 parts waterborne polyester modified unsaturated acrylate resin (model KDD704, purchased from Keding Company), 4 parts (meth)acrylate-2-hydroxyethyl ester, 3 parts α,α-diethoxyacetophenone, and 100 parts deionized water.

[0076] This embodiment provides a method for preparing the above-mentioned negative electrode slurry, which includes the following steps:

[0077] (1) The above-mentioned active material, conductive agent, water-based photocurable small molecule material and water-based photoinitiator are stirred to obtain a first mixture;

[0078] (2) Stir the first mixture obtained in step (1) and the water-based photocurable polymer material to obtain the second mixture. Then stir the second mixture and deionized water, filter and obtain the negative electrode slurry.

[0079] This embodiment also provides a negative electrode sheet and its preparation method, the preparation method is as follows:

[0080] The above-mentioned negative electrode slurry is coated on the surface of copper foil, and then subjected to ultraviolet light curing reaction to obtain a negative electrode sheet.

[0081] Example 6

[0082] The difference between this embodiment and Embodiment 1 is that the waterborne epoxy-modified unsaturated acrylate resin is replaced with waterborne epoxy resin, while all other aspects are the same as in Embodiment 1.

[0083] Comparative Example 1

[0084] The difference between this comparative example and Example 1 is that the weight of the waterborne epoxy-modified unsaturated acrylate resin is adjusted to 0.1 parts, while all other aspects are the same as in Example 1.

[0085] Comparative Example 2

[0086] The difference between this comparative example and Example 1 is that the weight of the waterborne epoxy-modified unsaturated acrylate resin is adjusted to 10 parts, while all other aspects are the same as in Example 1.

[0087] Comparative Example 3

[0088] The difference between this comparative example and Example 1 is that the weight of (meth)acrylate-2-hydroxyethyl ester is adjusted to 0.5 parts, while all other aspects are the same as in Example 1.

[0089] Comparative Example 4

[0090] The difference between this comparative example and Example 1 is that the weight of (meth)acrylate-2-hydroxyethyl ester is adjusted to 8 parts, while all other aspects are the same as in Example 1.

[0091] Application Examples 1 to 6 and Comparative Application Examples 1 to 4

[0092] Lithium-ion batteries were prepared using the negative electrode sheets provided in Examples 1 to 6 and Comparative Examples 1 to 4, and the preparation methods are as follows:

[0093] Preparation of lithium-ion batteries: The above-mentioned negative electrode, lithium metal, electrolyte and separator are assembled to obtain lithium-ion batteries.

[0094] Test conditions

[0095] The negative electrode sheets and lithium-ion batteries provided in Application Examples 1 to 6 and Comparative Application Examples 1 to 4 were tested using the following methods:

[0096] Electrode peel strength test: The prepared negative electrode sheet is cut into 20mm*200mm size and subjected to a 180° tensile test to test the adhesion between the negative electrode film and the foil.

[0097] Battery performance test: At room temperature, charge the battery to 4.2V with a constant current and constant voltage of 0.5C and cut off the current of 0.02C; then discharge it to 3.0V with a constant current of 0.5C and record the discharge capacity; repeat the above steps 1000 times; then measure the battery capacity retention rate.

[0098] The test results are shown in Table 1:

[0099] Table 1

[0100]

[0101]

[0102] As shown in Table 1, the negative electrode slurry provided by this invention does not require the use of organic solvents during the slurry preparation process. All its components are water-soluble materials, and deionized water is used as the dispersion medium, resulting in no significant pungent gas emissions and making it environmentally friendly. Furthermore, the negative electrode slurry provided by this invention utilizes ultraviolet light curing technology, enabling rapid cross-linking and curing, thus improving production efficiency.

[0103] Compared with Application Example 1, Application Example 6 shows that replacing the type of water-based polymer material cannot achieve the desired technical effect; Comparative Application Examples 1 to 4 show that this application enhances the adhesion between the binder and the powder, and between the electrode and the foil during the UV curing process by using components with specific contents, thereby effectively maintaining the stability of the battery.

[0104] The applicant declares that the present invention is illustrated by the above embodiments, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials used in the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A negative electrode slurry, characterized in that, The negative electrode slurry comprises the following components by weight: 80-95 parts of active material 1-5 parts of conductive agent 1-5 parts of water-based photocurable polymer material 1-4 parts of water-based light-curing small molecule material 0.1-3 parts of aqueous photoinitiator 20-100 parts deionized water; The waterborne photocurable polymer material is a waterborne polyester-modified unsaturated acrylate resin. The molecular weight of the waterborne polyester-modified unsaturated acrylate resin is 10,000 to 1,000,000. The waterborne photocurable small molecule material includes any one or a combination of at least two of the following: 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, ethoxyethoxyethyl acrylate, methoxy polyethylene glycol (meth)acrylate, dipropylene glycol diacrylate, triethylene glycol di(meth)acrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate, tetraethylene glycol dimethacrylate, or polyethylene glycol dimethacrylate.

2. The negative electrode slurry according to claim 1, characterized in that, The negative electrode slurry comprises the following components by weight: 85-92 parts of active material 1-5 parts of conductive agent 1-3 parts of water-based photocurable polymer material 1-2 parts of water-based photocurable small molecule material 0.1-2 parts of aqueous photoinitiator 50-100 parts deionized water.

3. The negative electrode slurry according to claim 2, characterized in that, The active material includes any one or a combination of at least two of the following: lithium titanate, titanium dioxide, graphite, mesophase carbon microspheres, elemental silicon, silicon oxides, or silicon alloys.

4. The negative electrode slurry according to claim 2, characterized in that, The average particle size of the active material is 5–20 μm.

5. The negative electrode slurry according to claim 4, characterized in that, The average particle size of the active material is 8–18 μm.

6. The negative electrode slurry according to claim 2, characterized in that, The conductive agent includes any one or a combination of at least two of carbon nanotubes, conductive carbon black, or graphene.

7. The negative electrode slurry according to claim 1, characterized in that, The molecular weight of the waterborne polyester-modified unsaturated acrylate resin is 50,000 to 800,000.

8. The negative electrode slurry according to claim 2, characterized in that, The aqueous photoinitiator is any one or a combination of at least two of the following: aqueous benzoin derivatives, aqueous acetophenone derivatives, or aqueous organophosphorus compounds.

9. A method for preparing a negative electrode slurry according to any one of claims 1-8, characterized in that, The method includes the following steps: (1) The active material, conductive agent, water-based photocurable small molecule material and water-based photoinitiator are mixed once to obtain the first mixture; (2) The first mixture obtained in step (1) is mixed with the water-based photocurable polymer material a second time to obtain the second mixture. Then the second mixture is mixed with deionized water a third time and filtered to obtain the negative electrode slurry.

10. The method according to claim 9, characterized in that, The mixing described in step (1) is carried out under stirring.

11. The method according to claim 9, characterized in that, The secondary and tertiary mixing in step (2) are both carried out under stirring.

12. A negative electrode sheet, characterized in that, The negative electrode sheet is prepared from the negative electrode slurry according to any one of claims 1-8.

13. A lithium-ion battery, characterized in that, The lithium-ion battery includes a positive electrode, a negative electrode, an electrolyte, and a separator, wherein the negative electrode is the negative electrode as described in claim 12.

Citation Information

Patent Citations

  • Preparation method of electrode slurry

    CN106920917A

  • Polyacrylate photo-curing adhesive and application thereof in silicon negative electrode plate of lithium ion battery

    CN111234119A