Uranium dioxide powder and its preparation method and application

By using the temperature switching of inert gas and reducing gas and the use of vertical resistance furnace in the preparation of UO2 powder, the safety risks and specific surface area control problems in the traditional decomposition and reduction process are solved, and safety and efficiency are improved. .

CN116253363BActive Publication Date: 2024-10-11NUCLEAR POWER INSTITUTE OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211489247.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-25
Publication Date
2024-10-11
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

The use of hydrogen in the decomposition and reduction process of traditional UO2 powder has safety risks, and it is difficult to control the specific surface area of ​​the powder, making it unable to meet user needs.

Method used

After using inert gas for drying and decomposition, switch to reducing gas for reduction, control temperature and atmosphere switching to adjust the specific surface area of ​​UO2 powder, and use a vertical resistance furnace instead of a rotary furnace to improve temperature uniformity and safety.

Benefits of technology

It achieves effective control of the specific surface area of ​​UO2 powder, improves process safety and equipment efficiency, and can prepare UO2 powder with specific specific surface area according to needs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a uranium dioxide powder and a preparation method and application thereof, and belongs to the field of nuclear fuel and material technology. The preparation method of uranium dioxide powder comprises: heating the ammonium diuranate powder made of high-fluorine material in an inert gas atmosphere for drying and decomposition, and then switching the inert gas to a reducing gas for reduction. The present invention provides a preparation method of uranium dioxide powder, wherein the ammonium diuranate powder obtained by re-dissolving the high-fluorine material through the diuranate ammonia method is decomposed and reduced to a uranium dioxide powder with uniform properties, and the specific surface area of ​​the obtained uranium dioxide powder can be effectively adjusted by regulating the inert gas / reducing gas switching temperature, and the existing decomposition and reduction process of ADU powder after re-dissolving the high-fluorine material can be optimized, so as to achieve the regulation of the specific surface area of ​​the powder and improve the process safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of nuclear fuel and material technology, and in particular to uranium dioxide powder and a preparation method and application thereof. Background Art

[0002] Uranium dioxide (UO 2 ) Pellets are an important form of nuclear fuel for reactors. 2 Fuel pellets are usually made by powder metallurgy, with UO 2 The physical and chemical properties of the powder, especially the specific surface area and oxygen-uranium ratio, will directly affect the final performance of the fuel pellet. 2 The powder method is ADU method, ADU method is used to prepare UO 2 Due to various abnormal conditions in the powder process, UO with fluorine content exceeding the technical requirements will be produced. 2 Powder (>150μg / g) is usually called high-fluorine material. The high-fluorine material is usually treated by the ADU return process, that is, the high-fluorine material is calcined to obtain uranium trioxide (U3O8). 3 O 8 ), then dissolved in nitric acid and extracted and purified to obtain uranyl nitrate solution, and then precipitated the uranium in the hydrolyzate in the form of ammonium diuranate (ADU) using a precipitant ammonia water, and then filtered and dried to obtain ADU powder, which was then decomposed and reduced to obtain UO 2 Powder. The traditional decomposition reduction is to use water vapor and hydrogen to pyrolyze and reduce ADU in a rotary kiln to obtain UO 2 Powder. Hydrogen is generally used throughout the decomposition and reduction process, which poses a high safety risk. 2 The specific surface area of ​​the powder is difficult to control, and it is impossible to prepare UO with a certain specific surface area according to user needs. 2 Powder; at the same time, a rotary kiln is used, the equipment structure is complex and the temperature uniformity is difficult to ensure. Summary of the invention

[0003] The present invention aims to provide a uranium dioxide powder and a preparation method and application thereof, which solves the problem that the traditional decomposition and reduction process of ADU powder uses hydrogen throughout the whole process, which has certain safety problems and is difficult to be used for UO 2 The problem of regulating the specific surface area of ​​powder according to demand.

[0004] The present invention is achieved through the following technical solutions:

[0005] The present invention provides a method for preparing uranium dioxide powder, comprising:

[0006] After the ammonium diuranate powder made of high-fluorine material is heated in an inert gas atmosphere for drying and decomposition, the inert gas is switched to a reducing gas for reduction.

[0007] Furthermore, in the preparation method of uranium dioxide powder, the step of preparing the high-fluorine material into ammonium diuranate powder is: defluorinating the high-fluorine material in (300-800)°C steam for (2-5) hours, and preparing the powder by reverse dissolution and precipitation with nitric acid.

[0008] Furthermore, in the method for preparing uranium dioxide powder, the conditions for drying and decomposing are:

[0009] In the first stage, the temperature is raised from room temperature to (200-300)°C and kept at this temperature for (1-2) hours;

[0010] In the second stage, the temperature is raised to (350-500)°C at a heating rate of (1-3)°C / min and kept at this temperature for (2-3h);

[0011] In the third stage, the temperature is raised to (600-800)°C.

[0012] Furthermore, in the method for preparing uranium dioxide powder, the inert gas includes argon, nitrogen or helium.

[0013] Furthermore, in the preparation method of uranium dioxide powder, the reduction conditions are: (600-800)°C, and heat preservation for (2-3h).

[0014] Furthermore, in the method for preparing uranium dioxide powder, the reducing gas includes: hydrogen, carbon monoxide or methane.

[0015] Furthermore, in the preparation method of uranium dioxide powder, the method also includes: after the reduced uranium dioxide powder is cooled to room temperature, nitrogen is introduced for (1-2) hours, and then air with a volume ratio of (5-15)% is introduced for (2-3) hours.

[0016] Furthermore, in the method for preparing uranium dioxide powder, the preparation of uranium dioxide powder is carried out in layers in a vertical resistance furnace.

[0017] The present invention also provides uranium dioxide powder prepared by the above-mentioned preparation method of uranium dioxide powder.

[0018] The present invention also provides application of the above uranium dioxide powder in nuclear fuel.

[0019] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0020] The invention provides a method for preparing uranium dioxide powder. The method comprises the following steps: the uranium dioxide powder is obtained by re-dissolving a high-fluorine material through a uranium dioxide ammonia method, and then the uranium dioxide ammonia powder is decomposed and reduced to obtain uranium dioxide powder with uniform properties. The specific surface area of ​​the obtained uranium dioxide powder can be effectively adjusted by regulating the inert gas / reducing gas switching temperature. The existing decomposition and reduction process of ADU powder after re-dissolving a high-fluorine material can be optimized, the specific surface area of ​​the powder can be regulated, and the process safety can be improved. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with Examples. The illustrative embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0022] The technical solution of the present invention is:

[0023] A method for preparing uranium dioxide powder, comprising:

[0024] (1) Using high-fluorine material as raw material, defluorinate the high-fluorine material in (300-800)°C steam for (2-5) hours, and then dissolve and precipitate using nitric acid to obtain ammonium diuranate powder. The high-fluorine material is defluorinated by steam calcination, and then dissolved in nitric acid to obtain ammonium diuranate powder. The steam can be selected from water vapor, or a mixture of water vapor and air, and the temperature of the steam is maintained at (300-800)°C.

[0025] (2) The prepared ammonium diuranate powder is loaded into a stainless steel boat and placed in a vertical resistance furnace in layers. The vertical resistance furnace is used to replace the traditional rotary furnace. The equipment has a simple structure and is heated more evenly in layers, which is more conducive to the reaction.

[0026] (3) The ammonium diuranate powder is heated in an inert gas atmosphere for drying and decomposition to obtain uranium trioxide. Under the protection of an inert gas atmosphere, the ammonium diuranate powder is heated and dried, and then further heated and decomposed into uranium trioxide. Inert gases include argon, nitrogen or helium, which are used as protective gases.

[0027] Among them, the conditions for drying and decomposition are:

[0028] In the first stage, the temperature is raised from room temperature to (200-300)°C and kept at this temperature for (1-2) hours;

[0029] In the second stage, the temperature is raised to (350-500)°C at a heating rate of (1-3)°C / min and kept at this temperature for (2-3h);

[0030] In the third stage, the temperature is raised to (600-800)°C.

[0031] In the first stage, the residual water in the ammonium diuranate powder is removed by heating, which plays a role in drying. In the second stage, the ammonium diuranate powder is decomposed into uranium trioxide (UO 3 ): The nitrate in the ammonium diuranate powder decomposes under heat to produce NH 3 , UO 3 Via NH 3 Reduction and high temperature pyrolysis to convert to uranium trioxide (U 3 O 8 ) powder. In the third stage, U 3 O 8 The powder gradually grows with the increase of temperature. 3 O 8 The specific surface area of ​​the powder is reduced and the temperature of this third stage remains the same as the temperature at which the reduction is carried out.

[0032] (4) Maintaining the temperature of the drying and decomposition in step (3), directly switching the inert gas to a reducing gas to reduce the uranium trioxide to uranium dioxide. The reducing gas includes hydrogen, carbon monoxide or methane.

[0033] The reduction conditions are: (600-800)°C, heat preservation (2-3h). The reduction temperature and the drying and decomposition temperature are in the same range and remain the same. When performing the reduction, maintain the drying and decomposition temperature of step (3) and directly switch the atmosphere by replacing the inert gas with a reducing gas. Before the atmosphere is switched, U 3 O 8 The particles gradually grow as the temperature rises, and the powder surface area decreases; after the atmosphere is switched, U 3 O 8 Rapidly reduced to UO 2 In this process, the powder particles shrink rapidly, thereby increasing the specific surface area. By controlling the temperature of the inert gas and reducing gas before reduction, the higher the temperature, the smaller the U before the atmosphere is switched. 3 O 8 The lower the specific surface area of ​​the powder, the more UO is generated after the atmosphere is switched. 2 The lower the specific surface area of ​​the powder, the more effective the final UO can be by controlling the temperature of the switching atmosphere. 2 The specific surface area of ​​the powder can be controlled to control the activity of the powder. This method can prepare a powder with a controllable specific surface area of ​​(3-7) m by controlling the temperature of the inert gas and the reducing gas ((600-800)℃). 2 UO in the range of / g 2 powder.

[0034] In order to improve the stability of the powder, the preparation method of the uranium dioxide powder further comprises: after the reduced uranium dioxide powder is cooled to room temperature, nitrogen is introduced for (1-2) hours, and then air with a volume ratio of (5-15)% is introduced for (2-3) hours. The nitrogen used is industrial nitrogen with a purity of 99.5%.

[0035] In the following examples, argon was used as the inert gas and oxygen was used as the reducing gas.

[0036] Embodiment 1:

[0037] The method for preparing uranium dioxide powder of this embodiment comprises:

[0038] The first step is defluorination and reverse dissolution: the high-fluorine material is pre-defluorinated in a mixture of air and water vapor at 300°C for 2 hours, and then reverse-dissolved with nitric acid to prepare ADU powder again;

[0039] The second step is powder loading: weigh the ADU powder, load it into a stainless steel boat, and place the loaded boats in a vertical resistance furnace;

[0040] The third step is to pass argon: evacuate the vacuum in the furnace to below 50Pa, maintain the pressure and observe for a period of time to ensure that the furnace is airtight. Open the argon valve, adjust the argon flowmeter to pass argon, and observe the vacuum pressure gauge. When the pressure gauge reaches normal pressure, open the argon valve and adjust the Ar flow rate to 5L / min;

[0041] The fourth step is dehydration and drying: the temperature is raised from room temperature to 200°C under argon atmosphere and kept for 2 hours;

[0042] Step 5: Decomposition: slowly increase the temperature from the dehydration temperature to 350°C at a heating rate of 1°C / min and keep it for 2h;

[0043] Step 6: Switch to hydrogen: Raise the temperature to 800°C and switch argon to hydrogen;

[0044] Step 7: Reduction: Keep warm for 2h under hydrogen atmosphere;

[0045] Step 8: Cool down the furnace. When the temperature inside the furnace is lower than 200°C, cut in argon gas at 5L / min, turn off hydrogen, and purge the furnace for 30 minutes. After the argon purge is completed, open the drain valve of the tail gas tank to discharge the water produced by the reduction.

[0046] Step 9: Powder stabilization: When the temperature drops to room temperature, first introduce industrial nitrogen (purity 99.5%) for 2 hours, then introduce 5% air for 2 hours, and take the powder out of the furnace after the temperature in the furnace drops to room temperature.

[0047] The UO obtained in this embodiment 2 The specific surface area of ​​the powder is 3.04m 2 / g, and the oxygen-uranium ratio is 2.04.

[0048] Embodiment 2:

[0049] The method for preparing uranium dioxide powder of this embodiment comprises:

[0050] The first step is defluorination and reverse dissolution: first, the high-fluorine material is pre-defluorinated in a mixture of air and water vapor at 600°C for 4 hours, and then reverse-dissolved with nitric acid to re-prepare ADU powder;

[0051] The second step is powder loading: weigh the ADU powder, load it into a stainless steel boat, and place the loaded boats in a vertical resistance furnace;

[0052] The third step is to pass argon: evacuate the vacuum in the furnace to below 50Pa, maintain the pressure and observe for a period of time to ensure that the furnace is airtight. Open the argon valve, adjust the argon flowmeter to pass argon, and observe the vacuum pressure gauge. When the pressure gauge reaches normal pressure, open the argon valve and adjust the Ar flow rate to 7L / min;

[0053] The fourth step is to remove water and dry: heat from room temperature to 240℃ and keep it for 2h under argon atmosphere;

[0054] The fifth step is decomposition: slowly increase the temperature from the dehydration temperature to 450°C at a heating rate of 2°C / min and keep it for 2h;

[0055] Step 6: Switch to hydrogen: Raise the temperature to 700°C and switch from argon to hydrogen;

[0056] Step 7: Reduction: Keep warm for 2h under hydrogen atmosphere;

[0057] Step 8: Cooling: When the furnace temperature is lower than 200°C, cut in argon gas at 7L / min, turn off hydrogen, and purge the furnace for 30 minutes. After the argon purge is completed, open the drain valve of the tail gas tank to discharge the water produced by the reduction;

[0058] Step 9: Powder stabilization: When the temperature drops to room temperature, first introduce industrial nitrogen (purity 99.5%) for 1 hour, then introduce 10% air for 2 hours, and take the powder out of the furnace after the temperature in the furnace drops to room temperature.

[0059] The UO obtained in this embodiment 2 The specific surface area of ​​the powder is 4.01m 2 / g, and the oxygen-uranium ratio is 2.03.

[0060] Embodiment 3:

[0061] The method for preparing uranium dioxide powder of this embodiment comprises:

[0062] The first step is defluorination and reverse dissolution: first, the high-fluorine material is pre-defluorinated in a mixture of air and water vapor at 800°C for 5 hours, and then reverse-dissolved with nitric acid to prepare ADU powder again;

[0063] The second step is powder loading: weigh the ADU powder, load it into a stainless steel boat, and place the loaded boats in a vertical resistance furnace;

[0064] The third step is to pass argon: evacuate the vacuum in the furnace to below 50Pa, maintain the pressure and observe for a period of time to ensure that the furnace is airtight. Open the argon valve, adjust the argon flowmeter to pass argon, and observe the vacuum pressure gauge. When the pressure gauge reaches normal pressure, open the argon valve and adjust the Ar flow rate to 7L / min;

[0065] The fourth step is dehydration and drying: the temperature is raised from room temperature to 300°C under argon atmosphere and kept for 1 hour;

[0066] The fifth step is decomposition: slowly increase the temperature from the dehydration temperature to 500°C at a heating rate of 3°C / min and keep it for 2h;

[0067] Step 6: Switch to hydrogen: Raise the temperature to 600°C and switch argon to hydrogen;

[0068] Step 7: Reduction: Keep warm for 2h under hydrogen atmosphere;

[0069] Step 8: Cooling: When the furnace temperature is lower than 200°C, cut in argon gas at 7L / min, turn off hydrogen, and purge the furnace for 30 minutes. After the argon purge is completed, open the drain valve of the tail gas tank to discharge the water produced by the reduction;

[0070] The ninth step is powder stabilization: when the temperature drops to room temperature, first introduce industrial nitrogen (purity 99.5%) for 2 hours, then introduce 15% air for 3 hours, and take the product out of the furnace after the temperature in the furnace drops to room temperature.

[0071] The UO obtained in this embodiment 2 The specific surface area of ​​the powder is 6.45m 2 / g, and the oxygen-uranium ratio is 2.01.

[0072] Example 4

[0073] The method for preparing uranium dioxide powder of this embodiment comprises:

[0074] The first step is defluorination and reverse dissolution: first, the high-fluorine material is pre-defluorinated in a mixture of air and water vapor at 600°C for 4 hours, and then reverse-dissolved with nitric acid to re-prepare ADU powder;

[0075] The second step is powder loading: weigh the ADU powder, load it into a stainless steel boat, and place the loaded boats in a vertical resistance furnace;

[0076] The third step is to pass argon: evacuate the vacuum in the furnace to below 50Pa, maintain the pressure and observe for a period of time to ensure that the furnace is airtight. Open the argon valve, adjust the argon flowmeter to pass argon, and observe the vacuum pressure gauge. When the pressure gauge reaches normal pressure, open the argon valve and adjust the Ar flow rate to 5L / min;

[0077] The fourth step is dehydration and drying: heating from room temperature to 300°C under argon atmosphere and keeping the temperature for 2h;

[0078] The fifth step is decomposition: slowly increase the temperature from the dehydration temperature to 450°C at a heating rate of 2°C / min and keep it for 2h;

[0079] Step 6: Switch to hydrogen: Raise the temperature to 800°C and switch argon to hydrogen;

[0080] Step 7: Reduction: Keep warm for 2h under hydrogen atmosphere;

[0081] Step 8: Cool down the furnace. When the temperature inside the furnace is lower than 200°C, cut in argon gas at 5L / min, turn off hydrogen, and purge the furnace for 30 minutes. After the argon purge is completed, open the drain valve of the tail gas tank to discharge the water produced by the reduction.

[0082] The ninth step is powder stabilization: when the temperature drops to room temperature, first introduce industrial nitrogen (purity 99.5%) for 2 hours, then introduce 10% air for 2 hours, and take the product out of the furnace after the temperature in the furnace drops to room temperature.

[0083] Get UO 2 Powder specific surface area 3.26m 2 / g, oxygen-uranium ratio 2.08.

[0084] Example 5

[0085] The preparation method of uranium dioxide powder in this embodiment is consistent with that in embodiment 4, except that in the sixth step, the temperature is raised to 700°C.

[0086] This example obtains UO 2 Powder specific surface area 4.64m 2 / g, oxygen-uranium ratio 2.04.

[0087] Example 6

[0088] The preparation method of uranium dioxide powder in this embodiment is consistent with that in embodiment 4, except that in the sixth step, the temperature is raised to 600°C.

[0089] This example obtains UO 2 Powder specific surface area 6.76m 2 / g, oxygen-uranium ratio 2.08.

[0090] The data results of Examples 4-6 show that the higher the argon / hydrogen switching temperature, the higher the UO2 The lower the specific surface area of ​​the powder, the more effective the UO obtained can be adjusted by regulating the inert gas / reducing gas switching temperature. 2 Powder specific surface area.

[0091] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing uranium dioxide powder, characterized in that: include: After the ammonium diuranate powder made of high-fluorine material is heated in an inert gas atmosphere for drying and decomposition, the inert gas is switched to a reducing gas for reduction; The step of preparing the ammonium diuranate powder from the high-fluorine material is as follows: defluorinating the high-fluorine material in steam at (300-800)°C for (2-5) hours, and then dissolving and precipitating the high-fluorine material through nitric acid; The conditions for dry decomposition are: In the first stage, the temperature is raised from room temperature to (200~300)℃ and kept at this temperature for (1~2)h; In the second stage, the temperature is raised to (350-500)°C at a heating rate of (1-3)°C / min and kept at this temperature for (2-3h); The third stage, heating to (600~800)℃; The reduction conditions are: (600~800)℃, keep warm (2~3h); The reducing gas is hydrogen.

2. The method for preparing uranium dioxide powder according to claim 1, characterized in that: The inert gas includes argon, nitrogen or helium.

3. The method for preparing uranium dioxide powder according to any one of claims 1 to 2, characterized in that: The method further comprises: after the reduced uranium dioxide powder is cooled to room temperature, nitrogen is introduced for (1-2) hours, and then air with a volume ratio of (5-15)% is introduced for (2-3) hours.

4. The method for preparing uranium dioxide powder according to claim 3, characterized in that: The preparation of the uranium dioxide powder is carried out in layers in a vertical resistance furnace.

5. Uranium dioxide powder obtained by the method for preparing uranium dioxide powder according to any one of claims 1 to 4.

6. Use of the uranium dioxide powder according to claim 5 in nuclear fuel.