A wheel disc forging for a gas turbine compressor and a preparation method thereof

By optimizing the material composition and heat treatment process of the wheel forgings, the problem of difficulty in balancing strength and toughness and plasticity in the existing technology is solved, and the synergistic effect of high strength and low toughness-to-brittle transition temperature is achieved to meet the high-temperature performance requirements of gas turbines.

CN116262963BActive Publication Date: 2024-10-11SHENZHEN HIRISUN TECH INC
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202211658265.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-10-11
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

Existing wheel disc forgings for gas turbine compressors cannot meet the requirements of high strength and toughness and plasticity at the same time, and the ductile-to-brittle transition temperature is high and the residual stress is also large, which cannot meet the high-temperature tensile and durable performance requirements of gas turbines.

Method used

By optimizing the material element chemical composition ratio of wheel forgings, strictly controlling the content of harmful elements, adding Nb and Ta elements to improve the grain boundary strengthening effect of the alloy, and adopting step heating and multiple heat treatment processes, including preparatory heat treatment and performance heat treatment , quenching and tempering treatment to improve the structure of the forging and reduce residual stress.

Benefits of technology

It achieves high strength, good mechanical properties and low ductile-brittle transition temperature of the forging, meets the requirements for use of wheel disc forgings for gas turbine compressors, and ensures the toughness, plasticity and high-temperature performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116262963B_ABST
    Figure CN116262963B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wheel disc forgings, and discloses a wheel disc forging for a gas turbine compressor and a preparation method thereof. The raw material components of the wheel disc forgings include, by weight percentage: C: 0.20-0.43%, Si≤0.15%, Mn≤1.05%, Ni: 0.50-1.00%, Cr: 1.95-2.60%, Mo: 0.85-1.15%, V: 0.16-0.30%, Nb+Ta: 0.03-0.11%, Al≤0.020%, P≤0.017%, S≤0.017%, Sb≤0.017%, Cu≤0.15%, Sn≤0.017%, As≤0.020%, and the rest is Fe element. The invention can meet the use requirements of the wheel disc forging for a gas turbine compressor through a reasonable ratio of the chemical composition of the wheel disc material elements and a reasonable forging and heat treatment process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of wheel disc forgings, and in particular to a wheel disc forging for a gas turbine compressor and a preparation method thereof. Background Art

[0002] Gas turbines are the "crown jewel" of the equipment manufacturing industry, representing the highest level of high-end manufacturing. With the advantages of fast start-up speed, high efficiency, and low emissions, gas turbines have become one of the core power equipment of efficient energy systems. Especially under the goal of "carbon peak and carbon neutrality", my country's gas turbine industry will surely usher in rapid development, and the corresponding supporting casting and forging industry has broad market prospects.

[0003] The material of the wheel forging for gas turbine compressor is medium carbon chromium nickel molybdenum vanadium steel, which has strict mechanical property requirements. The difficulty of this wheel forging is to meet the high strength index while ensuring the toughness and plasticity requirements of the material, and to meet the high temperature tensile and long-lasting performance while meeting the low toughness-brittle transition temperature. In addition, the finished forging is required to have low residual stress. Therefore, in view of the strict performance requirements of the wheel forging for gas turbine compressor, it is urgent to develop a new forging material and preparation method to meet the high performance requirements of the wheel for gas turbine compressor.

[0004] The Chinese invention patent with publication number CN 102719761 B discloses a wheel forging and manufacturing process, which belongs to the field of mechanical manufacturing technology. The process further optimizes the material composition, controls the upper limit of the C and Mn element content, increases the Ni element content, reduces the P and S harmful element content, and reduces the Si content to reduce the temper brittleness with the Mn element; adds the electroslag remelting process to improve the purity of the molten steel, and further homogenizes the material and refines the grains through two normalizing treatments after forging heat treatment; its raw material components are: C, Mn, Si, P, S, Cr, Ni, Al, Cu, Fe. Although the wheel forging can meet the strength index and good mechanical properties, it cannot have a low toughness-brittleness transition temperature at the same time, and the toughness-plasticity requirements of the material cannot be met. Summary of the invention

[0005] In order to solve the technical problem of making the wheel forging meet the high strength index while ensuring the toughness and plasticity requirements of the material, the present invention provides a wheel forging for a gas turbine compressor and a preparation method thereof. Through a reasonable chemical composition ratio of the wheel material elements, the content of harmful elements is strictly controlled, and then through a reasonable forging and heat treatment process, the forging material performance can meet the use requirements of the wheel forging for a gas turbine compressor.

[0006] The specific technical scheme of the present invention is:

[0007] In a first aspect, the present invention provides a wheel forging for a gas turbine compressor. The raw material components of the wheel forging include, by weight percentage: C: 0.20-0.43%, Si≤0.15%, Mn≤1.05%, Ni: 0.50-1.00%, Cr: 1.95-2.60%, Mo: 0.85-1.15%, V: 0.16-0.30%, Nb+Ta: 0.03-0.11%, Al≤0.020%, P≤0.017%, S≤0.017%, Sb≤0.017%, Cu≤0.15%, Sn≤0.017%, As≤0.020%, and the rest are Fe elements.

[0008] The present invention strictly controls the content of harmful elements, controls the upper limit of the content of C, Si and Mn elements, appropriately increases the content of Ni element, and adds appropriate amounts of Nb and Ta to further improve the grain boundary strengthening effect of the alloy through reasonable chemical composition ratio of wheel disc material elements. Therefore, the wheel disc forging obtained can meet the strength index and good mechanical properties, and has a lower toughness-brittleness transition temperature, meeting the toughness-plasticity requirements of the material.

[0009] Preferably, the weight percentage of the Nb element is 0.01-0.08%; the weight percentage of the Ta element is 0.02-0.08%.

[0010] In a second aspect, the present invention further provides a method for preparing a wheel disc forging for a gas turbine compressor, comprising the following steps:

[0011] (1) The raw material components of the wheel disc forging are melted into a steel ingot, and the steel ingot is step-heated and forged to obtain a wheel disc forging blank; (2) The wheel disc forging blank is subjected to a preliminary heat treatment, which includes a normalizing treatment and a first tempering treatment in sequence; the preliminary heat treatment is mainly to improve the internal structure of the forging, refine the grains and reduce the residual stress, so as to prepare for the performance heat treatment.

[0012] (3) The blank obtained in step (2) is subjected to rough machining, and then subjected to performance heat treatment, wherein the performance heat treatment includes sequential quenching treatment and a second tempering treatment, and finally a wheel disc forging is obtained.

[0013] The raw material components are subjected to optimized forging and heat treatment processes, and the forging material properties are as follows: room temperature tensile strength Rm ≥ 855MPa, yield strength Rp0.2 ≥ 700MPa, elongation A ≥ 12%, section shrinkage Z ≥ 45%, impact performance KV2 greater than ≥ 41J, hardness HBW255 ~ 303; ductile-brittle transition temperature FATT50 ≤ -11 ° C; 400 ° C tensile strength Rm ≥ 690MPa, yield strength Rp0.2 ≥ 580MPa, elongation A ≥ 12%, section shrinkage Z ≥ 45%; endurance time at 500 ° C, 428MPa ≥ 100h; residual stress of finished forgings ≤ 59MPa. It meets the use requirements of wheel forgings for gas turbine compressors.

[0014] The preliminary heat treatment is mainly to improve the internal structure of the forging, refine the grains and reduce the residual stress, so as to prepare for the performance heat treatment. The performance heat treatment includes the quenching treatment and the second tempering treatment in sequence. The martensite structure is obtained by quenching to improve the strength of the forging, and then the uniform tempered troostite is obtained by tempering, so that the forging has excellent comprehensive mechanical properties, and has good plasticity and toughness while maintaining high strength.

[0015] Preferably, the normalizing treatment is: first heating to 200-300°C, keeping warm for 2-4h; then heating to 700-720°C at a heating rate of ≤80°C / h, keeping warm for 2-4h; then heating to 900-990°C at a heating rate of ≤80°C / h, keeping warm for 10-20h, then taking out of the furnace and air cooling to room temperature.

[0016] Austenitization is carried out through normalizing treatment, and then the sorbite structure is obtained by cooling, which can improve the internal structure of the forging and refine the grains. The step heating method is mainly used to prevent the increase of stress due to excessive heating, which may cause defects such as cracking of the forging.

[0017] Preferably, the first tempering treatment is: first heating to 200-300°C, keeping warm for 2-4h; then heating to 640-660°C, keeping warm for 10-20h; then cooling with the furnace to ≤200°C, and then air-cooling to room temperature.

[0018] The first tempering treatment is mainly to reduce residual stress and lay a good foundation for performance heat treatment.

[0019] Preferably, the quenching treatment is: first heating to 200-300°C, keeping warm for 2-4h; then heating to 700-720°C at a heating rate of ≤60°C / h, keeping warm for 2-4h; then heating to 910-950°C at a heating rate of ≤60°C / h, keeping warm for 4-10h, and then taking out of the furnace and water cooling to room temperature.

[0020] The austenite is fully homogenized by quenching, and then the forging is fully hardened by water cooling to obtain more martensitic structure, ensuring the high strength performance of the forging.

[0021] Preferably, the second tempering treatment is: first heating to 150-200°C, keeping warm for 2-4h; then heating to 640-660°C, keeping warm for 15-30h; then cooling with the furnace to ≤200°C, and then air-cooling to room temperature.

[0022] Uniform tempered troostite is obtained through high temperature tempering, which makes the forgings have excellent comprehensive mechanical properties, and has good plasticity and toughness while maintaining high strength, ensuring a low ductile-brittle transition temperature of the forgings.

[0023] Preferably, in step (1), the stepwise heating is as follows: placing the steel ingot in a heating furnace and heating it to 840-870°C, keeping it warm for 4-6 hours, and then continuing to heat it to 1250-1280°C and keeping it warm for 1-2 hours.

[0024] Preferably, the forging includes four forgings, the first forging is to press the steel ingot, chamfer, and cut the water nozzle; the second forging is to upset and stretch the steel ingot; the third forging is to round the steel ingot and cut it according to the required size of the wheel disc; the fourth forging is to upset and expand the steel ingot to obtain the required size of the wheel disc forging blank.

[0025] Preferably, the temperature during forging is 840-1280°C; when the temperature of the steel ingot is lower than 850°C, the steel ingot needs to be heated to 1250-1280°C in a heating furnace and kept warm for 1-2 hours before continuing forging. The upsetting deformation during the second forging process is 10%-60%, and the drawing deformation is 20%-80%.

[0026] By upsetting and drawing, the coarse cast structure is broken, the structure is refined and uniform, and defects such as shrinkage holes, looseness and pores are forged, thereby improving the internal quality of the forgings.

[0027] Compared with the prior art, the present invention has the following beneficial effects: through reasonable chemical composition ratio of wheel material elements, the harmful element content is strictly controlled, and through reasonable forging and heat treatment processes, the forging material performance can meet the use requirements of wheel forgings for gas turbine compressors. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a heat treatment curve diagram of the wheel disc forging for gas turbine compressor;

[0029] Figure 2 The forging process diagram of the wheel disc forging for gas turbine compressor is shown in FIG.

[0030] Figure 3 This is a schematic diagram of the finished product of the wheel forging for a gas turbine compressor. DETAILED DESCRIPTION

[0031] The present invention will be further described below in conjunction with the embodiments.

[0032] Example 1

[0033] The raw material composition of a wheel disc forging for a gas turbine compressor is shown in Table 1:

[0034] Table 1

[0035]

[0036] The weight percentage of the Nb element is 0.02%; the weight percentage of the Ta element is 0.03%.

[0037] The method for preparing the above-mentioned wheel disc forging for a gas turbine compressor comprises the following steps:

[0038] (1) The raw material components of the wheel forging are produced into steel ingots according to the vacuum carbon deoxidation smelting method, and the steel ingots are heated step by step. The steel ingots are placed in a heating furnace and heated to 845°C. After being kept warm for 4 hours, they are further heated to 1260±10°C and kept warm for 1 hour. Four more forgings are performed, and the temperature during forging is maintained at 840-1280°C. When the temperature of the steel ingot is lower than 850°C, the steel ingot needs to be heated to 1250-1280°C in a heating furnace and kept warm for 1-2 hours. Figure 2 As shown, the first forging is to press the steel ingot, chamfer the edges, and cut off the nozzle; the second forging is to upset and stretch the steel ingot, with the upset deformation being 15% and the stretch deformation being 70%; the third forging is to round the steel ingot and cut it into the required size of the wheel disc; the fourth forging is to upset and expand the steel ingot to obtain the wheel disc forging blank according to the required size.

[0039] (2) Figure 1 As shown, the wheel disc forging blank is subjected to preliminary heat treatment, which includes normalizing treatment and first tempering treatment in sequence:

[0040] Normalizing: first heat to 250±10℃, keep warm for 2h; then heat to 710±5℃ at a heating rate of 50℃ / h, keep warm for 2h; then heat to 910±5℃ at a heating rate of 70℃ / h, keep warm for 10h, then take out of the furnace and air cool to room temperature;

[0041] First tempering: first heat to 250±10℃, keep warm for 2h; then heat to 650±5℃, keep warm for 10h; then cool to 150℃ in the furnace, then take out of the furnace and air cool to room temperature.

[0042] (3) The blank obtained in step (2) is subjected to rough machining, and then subjected to performance heat treatment, wherein the performance heat treatment includes a quenching treatment and a second tempering treatment performed in sequence:

[0043] Quenching: first heat to 210±10℃, keep warm for 2h; then heat to 710±5℃ at a heating rate of 45℃ / h, keep warm for 2h; then heat to 915±5℃ at a heating rate of 40℃ / h, keep warm for 4h, then take out of the furnace and water cool to room temperature;

[0044] Second tempering: first heat to 160±10℃, keep warm for 2h; then heat to 645±5℃ at a heating rate of 35℃ / h, keep warm for 15h; then cool to 150℃ at a cooling rate of 10℃ / h, then take out of the furnace and air cool to room temperature.

[0045] like Figure 3 Shown is a schematic diagram of the finished product of a wheel forging for a gas turbine compressor.

[0046] Example 2

[0047] The raw material composition of a wheel disc forging for a gas turbine compressor is shown in Table 2:

[0048] Table 2

[0049]

[0050] The weight percentage of the Nb element is 0.03%; the weight percentage of the Ta element is 0.04%.

[0051] The method for preparing the above-mentioned wheel disc forging for a gas turbine compressor comprises the following steps:

[0052] (1) The raw material components of the wheel disc forging are produced into a steel ingot according to the vacuum carbon deoxidation smelting method, and the steel ingot is heated stepwise. The steel ingot is placed in a heating furnace and heated to 845°C. After being kept warm for 4 hours, it is further heated to 1260±10°C and kept warm for 1 hour. Four more forgings are performed, and the temperature during forging is maintained at 840-1280°C. When the temperature of the steel ingot is lower than 850°C, the steel ingot needs to be placed in a heating furnace and heated to 1250-1280°C and kept warm for 1-2 hours. The first forging is to press the steel ingot, chamfer the edges, and cut off the water nozzle. The second forging is to upset and stretch the steel ingot, with an upset deformation of 30% and a stretch deformation of 60%. The third forging is to round the steel ingot and cut it according to the required size of the wheel disc. The fourth forging is to upset and expand the steel ingot to obtain a wheel disc forging blank according to the required size.

[0053] (2) The wheel disc forging blank is subjected to preliminary heat treatment, and the preliminary heat treatment includes normalizing treatment and first tempering treatment performed in sequence:

[0054] Normalizing: first heat to 250±10℃, keep warm for 2h; then heat to 710±5℃ at a heating rate of 55℃ / h, keep warm for 2.5h; then heat to 920℃ at a heating rate of 65℃ / h, keep warm for 13h, then take out of the furnace and air cool to room temperature;

[0055] First tempering: first heat up to 250±10℃, keep warm for 3h; then heat up to 650±5℃, keep warm for 10h; then cool down to 160℃ in the furnace, then take out of the furnace and air cool to room temperature.

[0056] (3) The blank obtained in step (2) is subjected to rough machining, and then subjected to performance heat treatment, wherein the performance heat treatment includes a quenching treatment and a second tempering treatment performed in sequence:

[0057] Quenching: first heat to 280±10℃, keep warm for 2.5h; then heat to 710±10℃ at a heating rate of 50℃ / h, keep warm for 3h; then heat to 945±5℃ at a heating rate of 50℃ / h, keep warm for 5h, then take out of the furnace and water cool to room temperature;

[0058] Second tempering: first heat to 180±10℃, keep warm for 3h; then heat to 645±5℃ at a heating rate of 40℃ / h, keep warm for 20h; then cool to 180℃ at a cooling rate of 15℃ / h, then take out of the furnace and air cool to room temperature.

[0059] Comparative Example 1

[0060] The raw material composition of a wheel disc forging for a gas turbine compressor is shown in Table 3:

[0061] Table 3

[0062]

[0063] The preparation method of the above-mentioned wheel disc forging for gas turbine compressor adopts the same process as Example 1.

[0064] The steps include:

[0065] (1) The raw material components of the wheel disc forging are produced into a steel ingot according to the vacuum carbon deoxidation smelting method, and the steel ingot is step-heated. The steel ingot is placed in a heating furnace and heated to 845°C. After being kept warm for 4 hours, it is further heated to 1260±10°C and kept warm for 1 hour; four more forgings are performed, and the temperature during forging is maintained at 840-1280°C. When the temperature of the steel ingot is lower than 850°C, the steel ingot needs to be placed in a heating furnace and heated to 1250-1280°C and kept warm for 1-2 hours; the first forging is to press the steel ingot, chamfer the edges, and cut off the water nozzle; the second forging is to upset and stretch the steel ingot, and the upset deformation is 15% and the stretch deformation is 70%; the third forging is to round the steel ingot and cut it according to the required size of the wheel disc; the fourth forging is to upset and expand the steel ingot to obtain the wheel disc forging blank according to the required size.

[0066] (2) The wheel disc forging blank is subjected to preliminary heat treatment, and the preliminary heat treatment includes normalizing treatment and first tempering treatment performed in sequence:

[0067] Normalizing: first heat to 250±10℃, keep warm for 2h; then heat to 710±5℃ at a heating rate of 50℃ / h, keep warm for 2h; then heat to 910±5℃ at a heating rate of 70℃ / h, keep warm for 10h, then take out of the furnace and air cool to room temperature;

[0068] First tempering: first heat to 250±10℃, keep warm for 2h; then heat to 650±5℃, keep warm for 10h; then cool to 150℃ in the furnace, then take out of the furnace and air cool to room temperature.

[0069] (3) The blank obtained in step (2) is subjected to rough machining, and then subjected to performance heat treatment, wherein the performance heat treatment includes a quenching treatment and a second tempering treatment performed in sequence:

[0070] Quenching: first heat to 210±10℃, keep warm for 2h; then heat to 710±5℃ at a heating rate of 45℃ / h, keep warm for 2h; then heat to 915±5℃ at a heating rate of 40℃ / h, keep warm for 4h, then take out of the furnace and water cool to room temperature;

[0071] Second tempering: first heat to 160±10℃, keep warm for 2h; then heat to 645±5℃ at a heating rate of 35℃ / h, keep warm for 15h; then cool to 150℃ at a cooling rate of 10℃ / h, then take out of the furnace and air cool to room temperature.

[0072] Mechanical properties of the forgings obtained in Examples 1-2 and Comparative Example 1 were tested. The room temperature and high temperature tensile performance standards were respectively based on GB / T 228.1-2010 Tensile test for metal materials Part 1: Room temperature test method, GB / T 228.2-2015 Tensile test for metal materials Part 2: High temperature test method; the impact energy and ductile-brittle transition temperature tests were based on GB / T 229-2007 Charpy pendulum impact test method for metal materials; the hardness was based on GB / T 231.1-2018 Brinell hardness test for metal materials Part 1: Test method; the short-term endurance test was based on GB / T 2039-2012 Uniaxial tensile creep test method for metal materials; the residual stress was based on JB / T 8888-2018 Test method for measuring residual stress of turbine and turbogenerator rotor forgings by ring core method. The test results are shown in Tables 4 and 5.

[0073] Table 4

[0074]

[0075] Table 5

[0076] Forging performance Durability time at 500℃, 428MPa (h) Residual stress (MPa) Example 1 120 50 Example 2 135 45 Comparative Example 1 121 65

[0077] As shown in Tables 4-5, the forgings prepared in the present invention meet the requirements of the wheel disc forgings for gas turbine compressors, while the forgings of Comparative Example 1, although using the same production process as Example 1, have different chemical compositions, specifically, the C, Cr, Mo, and V elements exceed the specified upper limits, and no Nb and Ta elements are added, which results in an increase in the strength of the forgings, but the ductile-brittle transition temperature and residual stress are too high, failing to meet the technical requirements of the wheel disc forgings for gas turbine compressors. Only under the element ratio in the present invention can a better synergistic effect be achieved, so that the forging material properties can meet the use requirements of the wheel disc forgings for gas turbine compressors.

[0078] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a wheel disc forging for a gas turbine compressor, characterized in that: The steps include: (1) The raw material components of the wheel disc forging are melted into a steel ingot, and the steel ingot is step-heated and forged to obtain a wheel disc forging blank; the raw material components of the wheel disc forging include, by weight percentage: C: 0.20-0.43%, Si≤0.15%, Mn≤1.05%, Ni: 0.50-1.00%, Cr: 1.95-2.60%, Mo: 0.85-1.15%, V: 0.16-0.30%, Nb+Ta: 0.03-0.11%, Al≤0.020%, P≤0.017%, S≤0.017%, Sb≤0.017%, Cu≤0.15%, Sn≤0.017%, As≤0.020%, and the rest is Fe element; (2) The wheel forging blank is normalized by first heating to 200-300°C, keeping it warm for 2-4h, then heating to 700-720°C, keeping it warm for 2-4h, then heating to 900-990°C, keeping it warm for 10-20h, then taking it out of the furnace and air cooling it to room temperature; then the first tempering treatment is carried out by first heating to 200-300°C, keeping it warm for 2-4h, then heating to 640-660°C, keeping it warm for 10-20h, then cooling it with the furnace to ≤200°C, then taking it out of the furnace and air cooling it to room temperature; (3) The blank is subjected to rough machining and then quenching treatment, heating to 200-300°C, keeping warm for 2-4h, heating to 700-720°C, keeping warm for 2-4h, heating to 910-950°C, keeping warm for 4-10h, then taking out of the furnace and water cooling to room temperature; then a second tempering treatment is carried out, heating to 150-200°C, keeping warm for 2-4h, heating to 640-660°C, keeping warm for 15-30h, then cooling with the furnace to ≤200°C, then taking out of the furnace and air cooling to room temperature; finally, the wheel forging is obtained.

2. The preparation method according to claim 1, characterized in that: The weight percentage of the Nb element is 0.01-0.08%; the weight percentage of the Ta element is 0.02-0.08%.

3. The preparation method according to claim 2, characterized in that: The weight percentage of the Nb element is 0.02%; the weight percentage of the Ta element is 0.03%.

4. The preparation method according to claim 2, characterized in that: The weight percentage of the Nb element is 0.03%; the weight percentage of the Ta element is 0.04%.

5. The preparation method according to claim 1, characterized in that: The normalizing treatment is as follows: firstly heating to 200-300°C, keeping warm for 2-4h; then heating to 700-720°C at a heating rate of ≤80°C / h, keeping warm for 2-4h; then heating to 900-990°C at a heating rate of ≤80°C / h, keeping warm for 10-20h, and then taking out of the furnace and air cooling to room temperature.

6. The preparation method according to claim 1, characterized in that: The quenching treatment is as follows: firstly heating to 200-300°C, keeping warm for 2-4h; then heating to 700-720°C at a heating rate of ≤60°C / h, keeping warm for 2-4h; then heating to 910-950°C at a heating rate of ≤60°C / h, keeping warm for 4-10h, and then taking out of the furnace and cooling with water to room temperature.

7. The preparation method according to claim 1, characterized in that: In step (1), the stepwise heating is as follows: placing the steel ingot in a heating furnace and heating it to 840-870°C, keeping it warm for 4-6 hours, and then continuing to heat it to 1250-1280°C and keeping it warm for 1-2 hours.

8. The preparation method according to claim 1, characterized in that: The forging includes four forgings. The first forging is to press the steel ingot, chamfer the edges, and cut off the water nozzle; the second forging is to upset and stretch the steel ingot; the third forging is to round the steel ingot and cut it according to the required size of the wheel disc; the fourth forging is to upset and expand the steel ingot to obtain the required size of the wheel disc forging blank.

9. The preparation method according to claim 8, characterized in that: The temperature during forging is 840-1280° C.; the upsetting deformation during the second forging process is 10%-60%, and the drawing deformation is 20%-80%.

Citation Information

Patent Citations

  • Wheel disc forging and manufacturing method thereof

    CN102719761B

  • Manufacturing method of gear shaft forge piece for offshore drilling platform

    CN102029347A

  • Wheel disc forging and manufacturing method thereof

    CN102719761A

  • Ferritic stainless steel and manufacturing method for valve disc forge piece by using same

    CN104498843A

  • Manufacturing method of high-carbon and high-nickel alloy steel ring forgings for wind power generation