Antiviral finishing method for train bedding fabric

By using organic isothiazolinone antiviral finishing agents and chitosan modified finishing agents after pretreatment and ultrasonic cleaning, the problem of the spread of pathogenic microorganisms in train bedding fabrics during high-speed rail operations has been solved, and the antiviral effect and washability have been improved. sex, enhancing the ability to prevent and control viruses.

CN116263031BActive Publication Date: 2024-10-25HANGZHOU HUALI IND GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211570330.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2024-10-25
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

It is difficult to effectively control the spread of pathogenic microorganisms on train bedding fabrics during high-speed rail operation. Existing antiviral finishing agents have poor wash resistance during washing, affecting the antibacterial function.

Method used

After using pretreatment solution and ultrasonic cleaning, use organic isothiazolinone antiviral finishing agent for padding treatment, combined with chitosan and alkyd resin coating, modified antiviral finishing agent to improve antiviral effect and washability sex.

Benefits of technology

Significantly inhibits the growth and reproduction of viruses, enhances the prevention and control of infection sources, improves the antiviral effect and washability of fabrics, and prolongs the durability of the antiviral effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003987647340000091
    Figure BDA0003987647340000091
  • Figure BDA0003987647340000092
    Figure BDA0003987647340000092
  • Figure BDA0003987647340000093
    Figure BDA0003987647340000093
Patent Text Reader

Abstract

The present invention relates to the technical field of antiviral finishing methods, and discloses an antiviral finishing method for train bedding fabrics, comprising the following steps: (1) treating the fabric with a pretreatment solution, then ultrasonically cleaning it, and then drying it for standby use; (2) preparing an antiviral finishing agent into an aqueous solution with a concentration of 40 to 50 g / L, and padding the fabric in step (1) in the antiviral finishing solution, and then pre-drying and stentering and shaping it in sequence; the antiviral finishing agent is an organic isothiazolinone finishing agent or a modified antiviral finishing agent. The present invention prepares antiviral fabrics by padding train bedding fabrics with the antiviral finishing agent, and the antiviral effect on the surface of the fabrics is good, which can inhibit the growth and reproduction of viruses, further weaken the spread of germs and viruses, strengthen the prevention and control of infection sources, and reduce the harm of sudden and epidemic germs and viruses.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of antiviral finishing methods, and in particular to an antiviral finishing method for train bedding fabrics. Background Art

[0002] High-speed trains and other transportation vehicles play an increasingly important role in passenger transportation services. However, they are relatively closed, crowded, highly mobile, and have high ambient temperatures, which are particularly prone to cross-infection. In the environment we live in, there are a variety of pathogenic microorganisms, which refer to microorganisms that can invade the human body, cause infection or even infectious diseases, also known as pathogens. They are of various types and widely distributed, and can spread diseases through direct or indirect contact with the human body.

[0003] The main mechanisms of pathogenic microorganisms adsorbing on the surface are physical adsorption and electrostatic interaction. The amount of adsorption on the surface is a linear functional of the square root of time. Therefore, the longer it stays on the surface, the more likely it is to be strongly adsorbed on the surface, thereby attacking the human body. One strategy to reduce pathogen infection is to reduce the time of interaction between pathogenic microorganisms and materials, while another strategy is to make the material have surface properties that are unfavorable to viruses. For public places such as high-speed railways with large personnel flows and dense crowds, environmental disinfection is usually carried out before the train leaves the train, but effective and comprehensive control cannot be carried out during the long period of train operation, especially textiles such as train bedding that are in close contact with the human body and have a high probability of adsorbing pathogenic microorganisms, which are prone to cross-infection. Nowadays, with the increasing prominence of occupational diseases, chronic diseases, vector-borne organisms, infectious diseases and other diseases, it is necessary to strengthen the prevention and control of high-speed railway diseases, do a good job in the control, disinfection and inactivation of pathogenic microorganisms in the public environment, and promote the development of my country's railway public health.

[0004] The Chinese invention patent with publication number CN111851071A discloses an antiviral finishing agent, which includes the following components by weight: 30-50 parts of guanidine compounds; 10-20 parts of organosilicon quaternary ammonium salt compounds; 5-10 parts of metal salts; and 50-80 parts of water. However, although this type of antibacterial finishing agent can withstand washing with nonionic surfactants and cationic surfactants, most of the detergents used in daily life contain anionic surfactants. When the fabric is washed, the cationic quaternary ammonium salt bonded to the fiber surface is easy to combine with the anionic surfactant, which reduces or loses the antibacterial function of the fabric and has poor washing resistance. Summary of the invention

[0005] In order to solve the technical problem of improving the antiviral property of train bedding fabrics, the present invention provides an antiviral finishing method for train bedding fabrics, which can weaken the spread of germs and viruses, inhibit the growth and reproduction of viruses, strengthen the prevention and control of infection sources, and effectively control them during long periods of train operation to reduce the hazards of sudden and epidemic germs and viruses.

[0006] The specific technical solution of the present invention is: the present invention provides an antiviral finishing method for train bedding fabrics, comprising the following steps:

[0007] (1) treating the fabric with a pretreatment solution, then ultrasonically cleaning it, and then drying it for later use;

[0008] (2) The antiviral finishing agent is prepared into an aqueous solution with a concentration of 40 to 50 g / L, and the fabric in step (1) is immersed in the antiviral finishing solution, and then pre-dried and stretched to set the fabric; the antiviral finishing agent is an organic isothiazolinone finishing agent or a modified antiviral finishing agent.

[0009] The application and processing of antiviral finishing agents on textiles are mainly divided into fiber modification and post-finishing. Fiber modification is to combine traditional spinning methods with antiviral materials, and directly make antiviral fibers by blending antiviral materials with spinning solutions. However, it requires the antiviral finishing agent to have good dispersibility and spinnability, which will greatly affect the original quality of the fiber. Post-finishing usually refers to padding, impregnation or coating methods, among which padding and impregnation are more commonly used and simple to operate. The fabrics made by this method have significant antiviral effects and have little effect on the original properties of the fabric.

[0010] Isothiazolinone compounds are highly effective broad-spectrum fungicides, which mainly rely on the active part on the heterocyclic ring to form hydrogen bonds with the bases in the protein in the bacteria, adsorb on the bacterial cells, thereby destroying the structure in the cells and causing them to lose their replication ability, leading to cell death. The present invention prepares antiviral fabrics by padding train bedding fabrics with the antiviral finishing agent, and the antiviral effect on the surface of the fabric is good, which can inhibit the growth and reproduction of viruses, further weaken the spread of germs and viruses, strengthen the prevention and control of infection sources, and reduce the hazards of sudden and epidemic germs and viruses.

[0011] Preferably, in step (1), the pretreatment solution is a sodium dodecyl sulfate solution with a mass concentration of 0.4 to 0.8%.

[0012] Preferably, in step (1), the ultrasonic cleaning is performed using water with a bath ratio of 1:15 to 20.

[0013] Preferably, in step (2), the organic isothiazolinone finishing agent is one or more of 5-chloro-2-methyl-4-isothiazoline-3-one, 2-methyl-4-isothiazoline-3-one, 2-n-octyl-4-isothiazoline-3-one and 1,2-benzisothiazolin-3-one.

[0014] Preferably, the preparation method of the modified antiviral finishing agent comprises the following steps:

[0015] (a) dispersing chitosan in an aqueous solution of L-tartaric acid, and after ultrasonic treatment, adding concentrated sulfuric acid and placing the mixed solution in a reaction kettle, heating to 70-75° C. and stirring for reaction for 50-60 min; then adding 1,2-benzisothiazolin-3-one, heating to reflux for reaction for 2-3 h, and then rotary evaporating to obtain reactant I;

[0016] (b) Phthalic anhydride, isophthalic acid, pentaerythritol, trimethylolpropane, coconut oil, azobisisobutyronitrile and xylene are mixed and reacted at 140-150° C. for 4-5 hours, and water is removed; n-butanol is then added and stirred evenly, and the mixture is heated to 90-95° C., butyl titanate, silane coupling agent, nano-titanium dioxide and dibutyltin dilaurate are added, and the mixture is stirred and reacted for 5-6 hours; and then the mixture is distilled under reduced pressure to obtain reactant II;

[0017] (c) stirring the reactant II and simultaneously adding the reactant I dropwise to obtain a modified antiviral finishing agent.

[0018] The antiviral fabric obtained by the padding method has a good antiviral effect, but the durability and washability of its antiviral effect need to be further improved. The modified antiviral finishing agent in the present invention uses 1,2-benzisothiazolin-3-one as the main antiviral component, and is supplemented with chitosan to enhance the antiviral and antibacterial effects. After ultrasonic treatment of chitosan with acid, chitosan with a low molecular weight, high uniformity and good dispersibility can be obtained. At the same time, after grafting with L-tartaric acid, the content of hydroxyl and carboxyl groups can be effectively increased, and the hydrogen bond attraction between it and 1,2-benzisothiazolin-3-one is strengthened, which is conducive to the combination between 1,2-benzisothiazolin-3-one and chitosan, and improves stability and synergistic antiviral effects. Then it is coated with alkyd resin, which contains silver ion-doped nano titanium dioxide, which will absorb light quanta when exposed to light to excite the electrons in the valence band, forming electron-hole pairs, and then generating ·OH free radicals and superoxide ·O 2- , are strong oxidants that can attack the unsaturated bonds of organic matter or extract its hydrogen atoms, causing lipid decomposition. Therefore, it can not only kill bacteria and decompose them to achieve antibacterial and antiviral effects, but also release the internal antiviral components to achieve a better sustained release effect.

[0019] In addition, the alkyd resin coating can enhance the adhesion between the antiviral finishing agent and the fabric fibers, allowing it to penetrate into the fabric, improving the washability of the carpet. Coupled with the sustained-release effect, it reduces its dissolution rate during the carpet washing process and enhances the durability of its effect.

[0020] Preferably, in step (a), the viscosity of the chitosan is 200-300 mPa·s; the mass concentration of the aqueous solution of L-tartaric acid is 5-6%; the mass ratio of the chitosan, the aqueous solution of L-tartaric acid, concentrated sulfuric acid and 1,2-benzisothiazolin-3-one is 1:50:0.1:10-12; in step (c), the mass ratio of the reactant I to the reactant II is 1:9-10.

[0021] L-tartaric acid is also a good complexing agent with antioxidant and high temperature resistance properties, which can improve the stability of internal antiviral components. In addition, the viscosity of chitosan will affect its dispersibility and water solubility, as well as the effect of L-tartaric acid. The quality ratio of raw materials is related to the stability and sustained release effect of the modified antiviral finishing agent, which needs to be controlled and coordinated to achieve better results.

[0022] Preferably, in step (b), the mass ratio of phthalic anhydride, isophthalic acid, pentaerythritol, trimethylolpropane, coconut oil, azobisisobutyronitrile and xylene is 9-11: 1-2: 0.8-1.3: 15-18: 10-12: 0.04-0.05: 50; the mass ratio of n-butanol and coconut oil is 60-70: 0.1; the mass ratio of n-butanol, butyl orthotitanate, silane coupling agent, nano titanium dioxide and dibutyltin dilaurate is 60-70: 4-5: 0.5-0.7: 0.05-0.1: 0.05; the particle size of the nano titanium dioxide is not more than 50 nm.

[0023] Preferably, in step (2), the padding is performed at a bath ratio of 1:10-15 for 5-15 minutes, and the padding rate is 70-80%.

[0024] The bath ratio, padding ratio and the bonding between the antiviral finishing agent and the fabric are related, and the bonding is better within this range.

[0025] Preferably, in step (2), the pre-baking temperature is 100-105°C.

[0026] Preferably, in step (2), the stentering and shaping is performed at 170 to 175° C. for 25 to 35 seconds.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The antiviral fabric is prepared by padding the train bedding fabric with the antiviral finishing agent. The antiviral effect on the surface of the fabric is good, which can inhibit the growth and reproduction of viruses, further weaken the spread of germs and viruses, strengthen the prevention and control of infection sources, and reduce the harm of sudden and epidemic germs and viruses;

[0029] (2) The modified antiviral finishing agent has a good sustained-release antiviral effect and can also enhance its adhesion to fabric fibers, allowing it to penetrate into the fabric and improve the washability of the carpet. In addition, the sustained-release effect reduces its dissolution rate during the carpet washing process and enhances the durability of its effect. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with the embodiments.

[0031] Overall embodiment

[0032] An antiviral finishing method for train bedding fabrics comprises the following steps:

[0033] (1) treating the fabric with a sodium dodecyl sulfate solution having a mass concentration of 0.4-0.8%, then ultrasonically cleaning the fabric with water at a bath ratio of 1:15-20, and then drying the fabric for later use;

[0034] (2) The antiviral finishing agent is prepared into an aqueous solution with a concentration of 40 to 50 g / L, and the fabric in step (1) is immersed in the antiviral finishing solution at a bath ratio of 1:10 to 15 for 5 to 15 minutes, with a rolling rate of 70 to 80%, and then pre-dried at 100 to 105° C., and finally stretched and shaped at 170 to 175° C. for 25 to 35 seconds to obtain a train bedding fabric after antiviral finishing.

[0035] The antiviral finishing agent is an organic isothiazolinone finishing agent, specifically one or more of 5-chloro-2-methyl-4-isothiazoline-3-one, 2-methyl-4-isothiazoline-3-one, 2-n-octyl-4-isothiazoline-3-one and 1,2-benzisothiazolin-3-one.

[0036] Alternatively, the antiviral finishing agent is a modified antiviral finishing agent, and its preparation method comprises the following steps:

[0037] (a) dispersing chitosan with a viscosity of 200 to 300 mPa·s in an aqueous solution of L-tartaric acid with a mass concentration of 5 to 6%, ultrasonically treating for 30 to 40 minutes, adding concentrated sulfuric acid and placing the mixed solution in a reaction kettle, heating to 70 to 75° C. and stirring for reaction for 50 to 60 minutes; then adding 1,2-benzisothiazolin-3-one, heating to reflux for reaction for 2 to 3 hours, and then rotary evaporating to obtain reactant I; the mass ratio of chitosan, L-tartaric acid aqueous solution, concentrated sulfuric acid and 1,2-benzisothiazolin-3-one is 1:50:0.1:10 to 12;

[0038] (b) Phthalic anhydride, isophthalic acid, pentaerythritol, trimethylolpropane, coconut oil, azobisisobutyronitrile and xylene in a mass ratio of 9-11:1-2:0.8-1.3:15-18:10-12:0.04-0.05:50 are mixed and reacted at 140-150°C for 4-5 hours to remove water; n-butanol is then added and stirred evenly, wherein the mass ratio of n-butanol to coconut oil is 60-70:0.1; the mixture is heated to 90-95°C, butyl titanate, nano titanium dioxide (particle size not greater than 50 nm) and dibutyl tin dilaurate are added, and the mixture is stirred and reacted for 5-6 hours, wherein the mass ratio of n-butanol, butyl titanate, nano titanium dioxide and dibutyl tin dilaurate is 60-70:4-5:0.05-0.1:0.05; and then the mixture is distilled under reduced pressure to obtain reactant II;

[0039] (c) stirring the reactant II and simultaneously adding the reactant I dropwise, wherein the mass ratio of the reactant I to the reactant II is 1:9-10, to obtain a modified antiviral finishing agent.

[0040] Example 1

[0041] An antiviral finishing method for train bedding fabrics comprises the following steps:

[0042] (1) The fabric was treated with a sodium dodecyl sulfate solution with a mass concentration of 0.5% for 3 times, then rinsed with water, and then the fabric was ultrasonically cleaned in water for 10 minutes with a bath ratio of 1:20, and then dried in an electric blast drying oven at 100° C. for later use;

[0043] (2) 5-chloro-2-methyl-4-isothiazoline-3-one and water are mixed to prepare an antiviral finishing liquid with a concentration of 50 g / L, and the fabric in step (1) is immersed in the antiviral finishing liquid at a bath ratio of 1:15 for 10 min, with a rolling rate of 75%, and then pre-dried at 100° C., and finally stretched and shaped at 170° C. for 30 seconds to obtain a train bedding fabric after antiviral finishing.

[0044] Example 2

[0045] An antiviral finishing method for train bedding fabrics comprises the following steps:

[0046] (1) The fabric was treated with a sodium dodecyl sulfate solution with a mass concentration of 0.5% for 3 times, then rinsed with water, and then the fabric was ultrasonically cleaned in water for 10 minutes with a bath ratio of 1:20, and then dried in an electric blast drying oven at 100° C. for later use;

[0047] (2) The antiviral finishing agent is prepared into an aqueous solution with a concentration of 50 g / L, and the fabric in step (1) is immersed in the antiviral finishing solution at a bath ratio of 1:15 for 10 min, with a rolling rate of 75%, and then pre-dried at 100° C., and finally stretched and shaped at 170° C. for 30 seconds to obtain a train bedding fabric after antiviral finishing.

[0048] The antiviral finishing agent is a modified antiviral finishing agent, and its preparation method comprises the following steps:

[0049] (a) Chitosan with a viscosity of 260 mPa·s was dispersed in an aqueous solution of L-tartaric acid with a mass concentration of 6%, and after ultrasonic treatment for 35 minutes, concentrated sulfuric acid (mass concentration of 98%) was added and the mixed solution was placed in a reactor, heated to 75°C and stirred for 50 minutes; then, 1,2-benzisothiazolin-3-one was added, and the temperature was raised to reflux for 2 hours, wherein the mass ratio of chitosan, L-tartaric acid aqueous solution, concentrated sulfuric acid and 1,2-benzisothiazolin-3-one was 1:50:0.1:11; and then after rotary evaporation, reactant I was obtained;

[0050] (b) Phthalic anhydride, isophthalic acid, pentaerythritol, trimethylolpropane, coconut oil, azobisisobutyronitrile and xylene in a mass ratio of 10:1.6:1.3:15:10:0.05:50 are mixed and reacted at 150°C for 4 hours, and water is removed; n-butanol is then added and stirred evenly, and the mixture is heated to 95°C, and butyl titanate, nano titanium dioxide (average particle size of 30 nm) and dibutyl tin dilaurate are added, and the mixture is stirred and reacted for 5 hours, wherein the mass ratio of coconut oil, n-butanol, butyl titanate, nano titanium dioxide and dibutyl tin dilaurate is 0.1:60:5:0.1:0.05; and then vacuum distillation is performed to obtain reactant II;

[0051] (c) stirring the reactant II and simultaneously adding the reactant I dropwise, wherein the mass ratio of the reactant I to the reactant II is 1:10, to obtain a modified antiviral finishing agent.

[0052] Example 3

[0053] An antiviral finishing method for train bedding fabrics comprises the following steps:

[0054] (1) The fabric was treated with a sodium dodecyl sulfate solution with a mass concentration of 0.5% for 3 times, then rinsed with water, and then the fabric was ultrasonically cleaned in water for 10 minutes with a bath ratio of 1:20, and then dried in an electric blast drying oven at 100° C. for later use;

[0055] (2) The antiviral finishing agent is prepared into an aqueous solution with a concentration of 50 g / L, and the fabric in step (1) is immersed in the antiviral finishing solution at a bath ratio of 1:15 for 10 min, with a rolling rate of 75%, and then pre-dried at 100° C., and finally stretched and shaped at 170° C. for 30 seconds to obtain a train bedding fabric after antiviral finishing.

[0056] The antiviral finishing agent is a modified antiviral finishing agent, and its preparation method comprises the following steps:

[0057] (a) Chitosan with a viscosity of 300 mPa·s was dispersed in an aqueous solution of L-tartaric acid with a mass concentration of 5%, and after ultrasonic treatment for 40 minutes, concentrated sulfuric acid was added and the mixed solution was placed in a reactor, heated to 75°C and stirred for 60 minutes; then, 1,2-benzisothiazolin-3-one was added, and the temperature was raised to reflux for 2 hours, wherein the mass ratio of chitosan, L-tartaric acid aqueous solution, concentrated sulfuric acid and 1,2-benzisothiazolin-3-one was 1:50:0.1:10; and then after rotary evaporation, reactant I was obtained;

[0058] (b) Phthalic anhydride, isophthalic acid, pentaerythritol, trimethylolpropane, coconut oil, azobisisobutyronitrile and xylene in a mass ratio of 10:1.6:1.3:15:10:0.05:50 are mixed and reacted at 150°C for 4 hours, and water is removed; n-butanol is then added and stirred evenly, and the mixture is heated to 90°C, and butyl titanate, nano titanium dioxide (average particle size of 30 nm) and dibutyl tin dilaurate are added, and the mixture is stirred and reacted for 5 hours, wherein the mass ratio of coconut oil, n-butanol, butyl titanate, nano titanium dioxide and dibutyl tin dilaurate is 0.1:60:5:0.06:0.05; and then vacuum distillation is performed to obtain reactant II;

[0059] (c) stirring the reactant II and simultaneously adding the reactant I dropwise, wherein the mass ratio of the reactant I to the reactant II is 1:10, to obtain a modified antiviral finishing agent.

[0060] Example 4

[0061] An antiviral finishing method for train bedding fabrics comprises the following steps:

[0062] (1) The fabric was treated with a sodium dodecyl sulfate solution with a mass concentration of 0.5% for 3 times, then rinsed with water, and then the fabric was ultrasonically cleaned in water for 10 minutes with a bath ratio of 1:20, and then dried in an electric blast drying oven at 100° C. for later use;

[0063] (2) The antiviral finishing agent is prepared into an aqueous solution with a concentration of 50 g / L, and the fabric in step (1) is immersed in the antiviral finishing solution at a bath ratio of 1:15 for 10 min, with a rolling rate of 75%, and then pre-dried at 100° C., and finally stretched and shaped at 170° C. for 30 seconds to obtain a train bedding fabric after antiviral finishing.

[0064] The antiviral finishing agent is a modified antiviral finishing agent, and its preparation method comprises the following steps:

[0065] (a) Chitosan with a viscosity of 200 mPa·s was dispersed in an aqueous solution of L-tartaric acid with a mass concentration of 6%, and after ultrasonic treatment for 30 minutes, concentrated sulfuric acid was added and the mixed solution was placed in a reactor, heated to 75°C and stirred for 55 minutes; then, 1,2-benzisothiazolin-3-one was added, and the temperature was raised to reflux for 3 hours, wherein the mass ratio of chitosan, L-tartaric acid aqueous solution, concentrated sulfuric acid and 1,2-benzisothiazolin-3-one was 1:50:0.1:12; and then after rotary evaporation, reactant I was obtained;

[0066] (b) Phthalic anhydride, isophthalic acid, pentaerythritol, trimethylolpropane, coconut oil, azobisisobutyronitrile and xylene in a mass ratio of 9:1.2:1.3:18:12:50 are mixed and reacted at 150°C for 5 hours, and water is removed; n-butanol is then added and stirred evenly, and the mixture is heated to 95°C, and butyl titanate, nano titanium dioxide (average particle size of 40 nm) and dibutyl tin dilaurate are added and stirred for 5 hours, wherein the mass ratio of coconut oil, n-butanol, butyl titanate, nano titanium dioxide and dibutyl tin dilaurate is 0.1:60:4:0.06:0.05; and then vacuum distillation is performed to obtain reactant II;

[0067] (c) stirring the reactant II and simultaneously adding the reactant I dropwise, wherein the mass ratio of the reactant I to the reactant II is 1:9, to obtain a modified antiviral finishing agent.

[0068] Comparative Example 1

[0069] The difference from Example 2 is that L-tartaric acid is not added in the preparation method of the modified antiviral finishing agent.

[0070] The preparation method thereof comprises the following steps:

[0071] (a) Chitosan with a viscosity of 260 mPa·s was added to water, and then 1,2-benzisothiazolin-3-one was added, and the temperature was raised to reflux for reaction for 2 hours, wherein the mass ratio of chitosan, water and 1,2-benzisothiazolin-3-one was 1:50:11; and then after rotary evaporation, reactant I was obtained;

[0072] (b) Phthalic anhydride, isophthalic acid, pentaerythritol, trimethylolpropane, coconut oil, azobisisobutyronitrile and xylene in a mass ratio of 10:1.6:1.3:15:10:0.05:50 are mixed and reacted at 150°C for 4 hours, and water is removed; n-butanol is then added and stirred evenly, and the mixture is heated to 95°C, and butyl titanate, nano titanium dioxide (average particle size of 30 nm) and dibutyl tin dilaurate are added, and the mixture is stirred and reacted for 5 hours, wherein the mass ratio of coconut oil, n-butanol, butyl titanate, nano titanium dioxide and dibutyl tin dilaurate is 0.1:60:5:0.1:0.05; and then vacuum distillation is performed to obtain reactant II;

[0073] (c) stirring the reactant II and simultaneously adding the reactant I dropwise, wherein the mass ratio of the reactant I to the reactant II is 1:10, to obtain a modified antiviral finishing agent.

[0074] Comparative Example 2

[0075] The difference from Example 2 is that chitosan is not added in the preparation method of the modified antiviral finishing agent.

[0076] The preparation method thereof comprises the following steps:

[0077] (a) dispersing 1,2-benzisothiazolin-3-one in an aqueous solution of L-tartaric acid having a mass concentration of 6%, heating to reflux for 2 hours, wherein the mass ratio of the aqueous solution of L-tartaric acid to 1,2-benzisothiazolin-3-one is 50:11; and then subjecting to rotary evaporation to obtain reactant I;

[0078] (b) Phthalic anhydride, isophthalic acid, pentaerythritol, trimethylolpropane, coconut oil, azobisisobutyronitrile and xylene in a mass ratio of 10:1.6:1.3:15:10:0.05:50 are mixed and reacted at 150°C for 4 hours, and water is removed; n-butanol is then added and stirred evenly, and the mixture is heated to 95°C, and butyl titanate, nano titanium dioxide (average particle size of 30 nm) and dibutyl tin dilaurate are added, and the mixture is stirred and reacted for 5 hours, wherein the mass ratio of coconut oil, n-butanol, butyl titanate, nano titanium dioxide and dibutyl tin dilaurate is 0.1:60:5:0.1:0.05; and then vacuum distillation is performed to obtain reactant II;

[0079] (c) stirring the reactant II and simultaneously adding the reactant I dropwise, wherein the mass ratio of the reactant I to the reactant II is 1:10, to obtain a modified antiviral finishing agent.

[0080] Comparative Example 3

[0081] The difference from Example 2 is that in the preparation method of the modified antiviral finishing agent, the viscosity of chitosan is too high.

[0082] The preparation method thereof comprises the following steps:

[0083] (a) Chitosan with a viscosity of 400 mPa·s was dispersed in an aqueous solution of L-tartaric acid with a mass concentration of 6%, and after ultrasonic treatment for 35 minutes, concentrated sulfuric acid (mass concentration of 98%) was added and the mixed solution was placed in a reactor, heated to 75°C and stirred for reaction for 50 minutes; then, 1,2-benzisothiazolin-3-one was added, and the temperature was raised to reflux for reaction for 2 hours, wherein the mass ratio of chitosan, L-tartaric acid aqueous solution, concentrated sulfuric acid and 1,2-benzisothiazolin-3-one was 1:50:0.1:11; and then after rotary evaporation, reactant I was obtained;

[0084] (b) Phthalic anhydride, isophthalic acid, pentaerythritol, trimethylolpropane, coconut oil, azobisisobutyronitrile and xylene in a mass ratio of 10:1.6:1.3:15:10:0.05:50 are mixed and reacted at 150°C for 4 hours, and water is removed; n-butanol is then added and stirred evenly, and the mixture is heated to 95°C, and butyl titanate, nano titanium dioxide (average particle size of 30 nm) and dibutyl tin dilaurate are added, and the mixture is stirred and reacted for 5 hours, wherein the mass ratio of coconut oil, n-butanol, butyl titanate, nano titanium dioxide and dibutyl tin dilaurate is 0.1:60:5:0.1:0.05; and then vacuum distillation is performed to obtain reactant II;

[0085] (c) stirring the reactant II and simultaneously adding the reactant I dropwise, wherein the mass ratio of the reactant I to the reactant II is 1:10, to obtain a modified antiviral finishing agent.

[0086] Comparative Example 4

[0087] The difference from Example 2 is that in the preparation method of the modified antiviral finishing agent, no alkyd resin coating is used.

[0088] The preparation method thereof comprises the following steps:

[0089] (a) Chitosan with a viscosity of 260 mPa·s was dispersed in an aqueous solution of L-tartaric acid with a mass concentration of 6%. After ultrasonic treatment for 35 minutes, concentrated sulfuric acid (mass concentration of 98%) was added and the mixed solution was placed in a reactor, heated to 75°C and stirred for reaction for 50 minutes; then, 1,2-benzisothiazolin-3-one was added, and the temperature was raised to reflux for reaction for 2 hours, wherein the mass ratio of chitosan, L-tartaric acid aqueous solution, concentrated sulfuric acid and 1,2-benzisothiazolin-3-one was 1:50:0.1:11; after rotary evaporation, reactant I, i.e., a modified antiviral finishing agent, was obtained.

[0090] Performance Testing

[0091] Mechanical properties test: refer to the standards GB / T 3923.1 "Tensile properties of textile fabrics Part 1: Determination of breaking force and elongation at break (strip method)" and GB / T 3917.3 "Tear properties of textile fabrics Part 3: Determination of tear strength by trapezoidal method".

[0092] Antiviral performance test: refer to standard ISO 18184:2019 "Test for antiviral performance of textiles".

[0093] Antibacterial performance test: Reference standard GB / T20944-2007 "Evaluation of antibacterial properties of textiles".

[0094] Washing resistance test: Simulate the washing process at home, immerse the antiviral finished fabric in water, with a bath ratio of 1:50, a temperature of 25°C, and a washing time of 15 minutes, and measure the antiviral performance after washing 50 times.

[0095] Performance test under natural light: The antiviral finished fabric is placed under natural light conditions for 30 minutes to test its antibacterial and antiviral properties.

[0096] Table 1 Mechanical properties of train bedding fabrics after antiviral finishing

[0097]

[0098] Table 2 Antiviral properties of train bedding fabrics after antiviral finishing

[0099]

[0100] Table 3 Antiviral performance of train bedding fabrics under natural light

[0101]

[0102] As can be seen from Table 1, the antiviral finishing agent in the present invention has a good antiviral effect on the surface of the fabric, can inhibit the growth and reproduction of viruses, further weaken the spread of germs and viruses, strengthen the prevention and control of infection sources, reduce the hazards of sudden and epidemic germs and viruses, and the fabric can also have good mechanical properties after washing. In addition, the washability and durability after finishing with the modified antiviral finishing agent are better, which is more conducive to the use of train bedding fabrics. As can be seen from Tables 2-3, Comparative Example 1 shows that the lack of L-tartaric acid will result in a low degree of dispersion of chitosan, and will significantly reduce the load of 1,2-benzisothiazolin-3-one, reducing the antiviral effect. Comparative Example 2 shows that the lack of chitosan will also reduce the load of 1,2-benzisothiazolin-3-one, as well as the synergistic antiviral effect of chitosan itself. Comparative Example 3 shows that the viscosity of chitosan is too high, which will result in a low degree of dispersion, and the agglomeration of macromolecular chains will also reduce the load of 1,2-benzisothiazolin-3-one. Comparative Example 4 shows that the antiviral component has no sustained-release effect after being not coated with alkyd resin, and the antibacterial and antiviral effects will be reduced to a certain extent after long-term light treatment.

[0103] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. An antiviral finishing method for train bedding fabrics, characterized in that: The steps include: (1) treating the fabric with a pretreatment solution, then ultrasonically cleaning it, and then drying it for later use; (2) preparing an antiviral finishing agent into an aqueous solution with a concentration of 40-50 g / L, immersing the fabric in step (1) in the antiviral finishing solution, and then pre-drying and stentering the fabric for finalizing; The preparation of the antiviral finishing agent comprises: (a) Dispersing chitosan with a viscosity of 200-300 mPa·s in an aqueous solution of L-tartaric acid, after ultrasonic treatment, adding concentrated sulfuric acid and placing the mixed solution in a reactor, heating to 70-75°C and stirring for reaction for 50-60 min; then adding 1,2-benzisothiazolin-3-one, raising the temperature to reflux for reaction for 2-3 h, and then subjecting to rotary evaporation to obtain reactant I; (b) Phthalic anhydride, isophthalic acid, pentaerythritol, trimethylolpropane, coconut oil, azobisisobutyronitrile and xylene are mixed and reacted at 140-150°C for 4-5 hours, and water is removed; n-butanol is then added and stirred evenly, and the mixture is heated to 90-95°C, and butyl titanate, nano-titanium dioxide and dibutyltin dilaurate are added and stirred for 5-6 hours; and then vacuum distillation is performed to obtain reactant II; (c) Stirring the reactant II and simultaneously adding the reactant I dropwise to obtain an antiviral finishing agent.

2. The antiviral finishing method for train bedding fabrics according to claim 1, characterized in that: In step (1), the pretreatment solution is a sodium dodecyl sulfate solution with a mass concentration of 0.4-0.8%.

3. The antiviral finishing method for train bedding fabrics according to claim 1 or 2, characterized in that: In step (1), the ultrasonic cleaning is performed using water with a bath ratio of 1:15-20.

4. The antiviral finishing method for train bedding fabrics according to claim 1, characterized in that: In step (a), the viscosity of the chitosan is 200 mPa·s, 260 mPa·s or 300 mPa·s.

5. The antiviral finishing method for train bedding fabrics according to claim 1, characterized in that: In step (a), the mass concentration of the aqueous solution of L-tartaric acid is 5-6%; the mass ratio of the chitosan, the aqueous solution of L-tartaric acid, concentrated sulfuric acid and 1,2-benzisothiazolin-3-one is 1:50:0.1:10-12; in step (c), the mass ratio of the reactant I to the reactant II is 1:9-10.

6. The antiviral finishing method for train bedding fabrics according to claim 1, characterized in that: In step (b), the mass ratio of n-butanol to coconut oil is 60-70: 0.1; The mass ratio of n-butanol, butyl titanate, nano titanium dioxide and dibutyltin dilaurate is 60-70:4-5:0.05-0.1:0.05; the particle size of the nano titanium dioxide is not greater than 50nm.

7. The antiviral finishing method for train bedding fabrics according to claim 1, characterized in that: In step (2), the rolling process is as follows: the bath ratio is 1:10-15, the rolling time is 5-15 minutes, and the rolling rate is 70-80%.

8. The antiviral finishing method for train bedding fabrics according to claim 1, characterized in that: In step (2), the pre-baking temperature is 100-105°C.