A cuprous oxide / zinc oxide composite material and its preparation method and application

Preparation of Cu2O/ZnO composite materials by hydrothermal and chemical reduction methods solves the problems of low activity of existing photocatalysts and complex and high-cost preparation, achieves efficient catalytic conversion of benzene and CO2 into benzoic acid, simplifies experimental conditions and ensures Environmentally friendly and low cost.

CN116273010BActive Publication Date: 2024-10-25FUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310051088.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-02
Publication Date
2024-10-25
Estimated Expiration
2043-02-02

AI Technical Summary

Technical Problem

Existing photocatalysts have low activity in catalyzing the reaction between benzene and CO2, and the preparation process is complex and costly, involving precious metals and organic matter, which affects environmental protection.

Method used

Cu2O/ZnO composite materials were prepared by hydrothermal and chemical reduction methods, simplifying experimental conditions, avoiding polluting substances, using cheap and easily available raw materials, and uniformly dispersed through ultrasound and stirring to form 1% Cu2O/ZnO composite materials for photocatalysis.

Benefits of technology

The photocatalytic activity is improved, and efficient catalytic conversion of benzene and CO2 into benzoic acid is achieved. The experimental conditions are simple, the raw materials are environmentally friendly, the cost is low, and the catalyst activity is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116273010B_ABST
    Figure CN116273010B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of photocatalytic materials, and specifically relates to a cuprous oxide / zinc oxide composite material and its preparation method and application. ZnO is synthesized by a hydrothermal method, and then Cu2O is loaded on ZnO by a method of L-ascorbic acid reduction to obtain a Cu2O / ZnO composite material. The present invention synthesizes a zinc oxide-loaded cuprous oxide composite photocatalytic material by simple hydrothermal chemical reduction, and the raw materials for preparation are cheap and easy to obtain, do not contain precious metals and heavy metals that pollute the environment, and are used for photocatalytic reaction of benzene and carbon dioxide to prepare benzoic acid, which is a commonly used drug and preservative, and is also an important raw material in industrial production, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocatalytic materials, and specifically relates to a Cu2O / ZnO composite material, a preparation method thereof, and its effect on photocatalytically preparing benzoic acid from benzene and carbon dioxide. Background Art

[0002] The energy consumption and environmental climate change problems in the world today need to be solved urgently. The balance of CO2 production and consumption in nature has been gradually overturned by human beings' excessive use of fossil fuels in the past century. Exploring cheap and feasible CO2 conversion pathways has great fundamental and practical significance not only from the perspective of solving energy and environmental problems, but more importantly from the perspective of synthetic chemistry itself. There are many possible chemical pathways for converting and fixing CO2. In addition to direct hydrogenation reduction or reaction with water to convert into methane, alcohols, aldehydes, acids, etc., it can also be converted into higher-order organic compounds through redox reactions with various organic matter. The high thermodynamic barrier of CO2 is one of the main factors that make it difficult to reduce it efficiently. The thermodynamic barrier of the reaction between CO2 and benzene is not large, and benzoic acid, one of the possible products, is an important industrial raw material. It can not only solve environmental problems but also convert CO2 into high-value-added products, especially using semiconductor catalysts as photocatalysts to directly utilize and store solar energy. The key lies in finding a suitable and efficient catalyst.

[0003] In the process of semiconductor photocatalytic reaction, light irradiates the catalyst and the semiconductor material is excited by light. If the energy of the photon is greater than the bandgap width of the photocatalyst, the electrons and holes are separated, and the electrons in the valence band are excited and jump to the conduction band. At the same time, the holes are left in the valence band. Then the photogenerated electrons and holes migrate to the surface of the catalyst respectively and carry out redox half-reactions with the reactants, thus catalyzing CO2 and benzene to make the reaction occur. At present, there are many semiconductor materials that can be used as photocatalysts, but there are not many catalysts that can realize the photocatalytic reaction of benzene and CO2. ZnO is a very promising semiconductor photocatalytic material. It can be excited by sunlight and has a very positive valence band potential, which makes it have a strong redox ability. Our experiments have found that benzene and CO2 can be reacted by photocatalysis on this material. However, the photocatalytic activity of ZnO for benzene and CO2 is low, and the reaction efficiency needs to be further improved. There are many factors that affect this photocatalytic reaction, but in the previous extensive research on ZnO photocatalysts, the low separation efficiency of electrons and holes is one of the important factors that make its photocatalytic activity low. Loading precious metals or other non-metallic additives is considered to be one of the means to improve the efficiency of photogenerated electron-hole separation.

[0004] We found that the current synthesis of this type of material mostly has some problems, such as expensive raw material precious metals, complex synthesis process, and harsh synthesis conditions. Chinese patent CN106268874A discloses a gold / molybdenum sulfide / zinc oxide high-efficiency photocatalytic hydrogen production nanomaterial and its preparation method, which has a structure of gold nanoparticles as the core, molybdenum sulfide as the shell, and zinc oxide nanorods grown on the surface of molybdenum sulfide. However, its synthesis and preparation process is relatively complicated and the cost is relatively high, involving precious metal gold; Chinese patent CN107715859A discloses a preparation method of a graphene perovskite composite photocatalytic hydrogen production catalyst, comprising: weighing nitrate, tetrabutyl titanate and a complexing agent and dissolving them in an ethanol solution, adding a graphene suspension to prepare a mixed solution; stirring the mixed solution until it becomes a dry gel; calcining the dry gel to remove organic matter and then vacuum calcining to obtain the catalyst. The preparation of the catalyst involves some organic matter, and the preparation of graphene is relatively difficult and costly; Chinese patent CN108927222A discloses a method for preparing CdS-PAN / graphene composite nanofibers, but the preparation method is relatively complicated, the reaction conditions are relatively harsh, and the reaction involves CdS, heavy metals are involved, which is not environmentally friendly, and the preparation of graphene is relatively difficult and costly; Chinese patent CN101760272A discloses a preparation of a metal organic gel-loaded Pt catalyst and its application in photocatalytic hydrogen production, but the preparation conditions are relatively harsh, the cost of the Pt source is relatively high, and the organic matter involved in the reaction process is not environmentally friendly. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention aims to provide a Cu2O / ZnO composite material, a preparation method thereof, and its effect on the photocatalytic reaction of benzene and CO2 to generate benzoic acid. The preparation method has relatively simple experimental conditions, mainly through hydrothermal and simple chemical reduction, and does not involve environmentally polluting substances in the preparation process, and the raw materials are cheap and easy to obtain.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] A method for preparing a Cu2O / ZnO composite material for photocatalytically preparing benzoic acid from benzene and CO2 comprises the following steps:

[0008] 1) Weigh a certain mass of Zn(NO3)2·6H2O;

[0009] 2) Dissolve the weighed Zn(NO3)2·6H2O in a mixed solution of deionized water and ethanol, stir thoroughly, and fully dissolve;

[0010] 3) Adjust the pH of the solution with aqueous ammonia to prepare a milky white suspension.

[0011] 4) subjecting the suspension to a hydrothermal reaction, cooling, centrifuging, washing, drying, and calcining to obtain a ZnO material;

[0012] 5) Disperse a certain amount of ZnO in deionized water and stir by ultrasonic to disperse evenly.

[0013] 6) Add copper sulfate solution and sodium hydroxide solution dropwise into the ZnO suspension and stir to disperse.

[0014] 7) Adding L-ascorbic acid to the suspension prepared in 6), stirring to allow the reaction to proceed fully, centrifuging, washing, and drying to obtain a Cu2O / ZnO composite material.

[0015] Furthermore, the mass of Zn(NO3)2·6H2O in step 1) is 2.38 g (8 mmol).

[0016] Furthermore, in step 2), the volume ratio of deionized water to ethanol is 4:5, the total volume of the solution is 60 ml, and the stirring time is 30 min.

[0017] Furthermore, in step 3), the pH range adjusted by using aqueous ammonia is 8.0-8.3.

[0018] Furthermore, in step 4), the hydrothermal temperature is 160° C., the reaction time is 10 h, the drying treatment is ordinary drying at 60° C., the calcination temperature is 350° C., and the calcination time is 3 h.

[0019] Furthermore, in step 5), the mass of ZnO is 80 mg, and the ultrasonic time is 3 min.

[0020] Furthermore, in step 6), the concentrations of the CuSO4 solution and the NaOH solution are 0.05 M and 0.1 M, respectively, and the added amount is 250 μl each.

[0021] Furthermore, in step 7), the amount of L-ascorbic acid added is 100 mg, the stirring time is 20 min, and the drying method is vacuum drying at 60° C.

[0022] Furthermore, the present invention proposes that the 1% Cu2O / ZnO composite material prepared by the above method has the best activity in catalyzing the preparation of benzoic acid from benzene and CO2.

[0023] The photocatalytic activity of Cu2O / ZnO composites was tested by photocatalysis of benzene and CO2 systems under full-band lamp irradiation.

[0024] The physical properties of the Cu2O / ZnO composite photocatalytic material were characterized by using X-ray diffraction (XRD) spectroscopy to analyze the material composition and structure of the product, and using field emission scanning electron microscopy (FESEM) to observe the morphology of the product.

[0025] The advantages of the present invention are that the experimental conditions of the scheme are relatively simple, mainly through hydrothermal and simple chemical reduction methods, and the preparation process does not involve substances that pollute the environment, and the raw materials are easily available.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The invention synthesizes a Cu2O / ZnO composite material by a simple method. The raw materials for preparation are easily available and do not contain precious metals and heavy metals that pollute the environment. The composite material is used for photocatalytically preparing benzoic acid from benzene and CO2. Benzoic acid is a commonly used medicine and preservative, and is also an important raw material in industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the XRD spectrum of the Cu2O / ZnO composite material prepared by the synthesis method in Example 1.

[0029] Figure 2 This is the SEM photo of ZnO material.

[0030] Figure 3 This is a SEM photograph of the Cu2O / ZnO composite material prepared by the synthesis method in Example 1.

[0031] Figure 4 This is a diagram showing the effect of the catalyst obtained in Example 1 on producing benzoic acid.

[0032] Figure 5 This is a schematic diagram of the reactor for preparing benzoic acid by full-band photocatalysis of benzene and CO2 in Example 1. DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with embodiments, which are only used to illustrate the present invention and are not intended to limit the present invention.

[0034] Example 1

[0035] Under magnetic stirring, 2.38g Zn(NO3)2·6H2O was dissolved in 80ml of a mixed solution of anhydrous ethanol and deionized water with a volume ratio of 5:4 and stirred for 30 minutes. Subsequently, the pH of the solution was adjusted to 8.0-8.3 with ammonia water and stirred for 3h, and then the mixture was transferred to a stainless steel autoclave, sealed and kept at 160℃ for hydrothermal reaction for 10 hours, and then cooled to room temperature, and the wet precipitate was thoroughly washed and dried in an oven to obtain pure ZnO. 80mg of the prepared ZnO was weighed and dispersed in 80ml of deionized water, followed by adding 250μl 0.05MCuSO4 solution and 250μl 0.1M NaOH solution and stirring. Finally, 100mg L-ascorbic acid was added and stirred for 20min. The sample was collected by centrifugation and dried in a vacuum oven at 50℃ to obtain a 1wt% Cu2O / ZnO composite material. Using the same method, a series of composite materials with different loadings were obtained by changing the amount of CuSO4 solution and NaOH solution added.

[0036] From the XRD patterns of Cu2O / ZnO nanoparticles (such as Figure 1 ) It can be seen that the XRD pattern of the Cu2O / ZnO nanosheets synthesized by this method is completely consistent with the standard card of ZnO and does not contain other impurities. However, due to the low content of Cu2O, the characteristic peak of Cu2O is not clearly observed. From the ZnO material ( Figure 2 ) and SEM images of Cu2O / ZnO composites ( Figure 3 ) It can be seen that ZnO is a rod-shaped material with a length of 1-10 μm, and Cu2O is a spherical particle with a diameter of 100-500 nm. The Cu2O particles supported by the ZnO rod can be clearly observed. The effect diagram of the catalyst catalyzing benzene and CO2 to prepare benzoic acid ( Figure 4 ) It can be seen that the catalytic activity of ZnO after Cu2O loading is improved. The optimal loading amount of Cu2O is 1wt%. Under this condition, the catalyst sample synthesized has the best activity, and the efficiency of producing benzoic acid is 0.986μmol / (g·h). The production of benzoic acid by pure ZnO and Cu2O catalysts is relatively low or even negligible. The efficiency of photocatalytic production of benzoic acid by ZnO catalyst loaded with Cu2O is greatly improved. The reason is that after illumination, the photogenerated electrons generated by the Cu2O / ZnO composite material will be transferred to Cu2O, while the photogenerated holes will remain on ZnO, which reduces the recombination rate of photogenerated electrons and photogenerated charges and enhances the transfer ability and efficiency of photogenerated charges, thereby improving the redox ability of the catalyst. However, as the Cu2O loading increases (more than 1wt%), too much Cu2O catalyst will cover the active sites of ZnO itself and hinder the light absorption of ZnO.

[0037] Application Example 1

[0038] The specific steps of the experiment of preparing benzoic acid by photocatalysis of benzene and carbon dioxide are as follows:

[0039] The photocatalytic activity of the prepared Cu2O / ZnO composite samples was tested in Figure 5 The reaction is carried out in the reaction device shown, and the operating steps are as follows: 30 mg of the catalyst prepared by the present invention is placed in a weighing dish, and then evenly dispersed with a small amount of water, and then dried in an oven at 80° C. to form a catalyst film.

[0040] Then place the weighing dish containing the catalyst in the reactor, add 1 ml of benzene into the weighing dish, and then continuously introduce carbon dioxide gas into the reactor for 30 minutes. After the ventilation is completed, close the gas outlet and the gas inlet in turn. After irradiating with a 300W xenon light source for 120 minutes, add 5 ml of methanol into the reactor to absorb the generated benzoic acid, and use waters liquid chromatography to detect the content of benzoic acid in the reaction system. The entire reaction process is carried out at the same stirring speed (500r / s).

[0041] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. An application of a cuprous oxide / zinc oxide composite material in the photocatalytic preparation of benzoic acid from benzene and carbon dioxide, characterized in that: First, zinc oxide was synthesized by a hydrothermal method, and then cuprous oxide was deposited on zinc oxide in an aqueous solution to obtain a Cu2O / ZnO composite material.

2. The use according to claim 1, characterized in that: The specific preparation of the Cu2O / ZnO composite material comprises the following steps: 1) Weigh a certain amount of Zn(NO3)2·6H2O and dissolve it in a mixed solution of deionized water and anhydrous ethanol, then adjust the pH of the mixed solution with ammonia water; 2) subjecting the mixed solution to a hydrothermal reaction treatment, cooling, filtering, washing and drying to obtain ZnO; 3) Weigh a certain amount of ZnO, disperse it in water, add copper sulfate solution and sodium hydroxide solution and stir evenly, then add L-ascorbic acid and stir for 20 minutes, collect by centrifugation, and dry to obtain a Cu2O / ZnO composite material.

3. The use according to claim 2, characterized in that: In the step 1), the mass of Zn(NO3)2·6H2O weighed is 2.38 g, the volume of the solution is 60 mL, and the volume ratio of deionized water to anhydrous ethanol is 5:

4.

4. The use according to claim 2, characterized in that: In the step 1), the pH is adjusted to a range of 8.0-8.

3.

5. The use according to claim 2, characterized in that: In step 2), the hydrothermal temperature is 160° C. and the hydrothermal time is 10 h; the drying temperature is 60° C.

6. The use according to claim 2, characterized in that: Step 3) The concentrations of the copper sulfate solution and the sodium hydroxide solution are 0.05 M and 0.10 M, respectively.

7. The use according to claim 2, characterized in that: The mass of L-ascorbic acid added in step 3) is 100 mg.

8. The use according to claim 2, characterized in that: Step 3) Drying treatment is vacuum drying at a drying temperature of 50°C.