Polyethylene pipe for water supply and preparation method thereof

By adding polypropylene to polyethylene raw materials and performing specific heating and mixing processes, the problem of insufficient impact strength of polyethylene pipes is solved and its performance is significantly improved.

CN116285054BActive Publication Date: 2024-10-25HEBEI ZETIAN WATER SAVING TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211674095.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-10-25
Estimated Expiration
2042-12-26

Smart Images

  • Figure CN116285054B_ABST
    Figure CN116285054B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a polyethylene pipe for water supply, comprising the following steps: A. preparing raw materials, the raw materials comprising, the following parts are by mass, 200 parts of polyethylene, 3-5 parts of carbon black masterbatch, 1-2 parts of antioxidant, 1-2 parts of flame retardant, and 15 parts of polypropylene; B. putting polyethylene and polypropylene into an open mill for heating and mixing, standing and cooling for standby use; C. putting the polyethylene and polypropylene mixture treated in step B, as well as the carbon black masterbatch, antioxidant and flame retardant into a material cutter for mixing; D. inputting the mixed raw materials into an extruder for extrusion molding. The invention can solve the shortcomings of the prior art and improve the impact strength of the polyethylene pipe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer pipes, in particular to a polyethylene pipe for water supply and a preparation method thereof. Background Art

[0002] Polyethylene pipes are commonly used in water supply networks and have the advantages of corrosion resistance and durability. How to further improve the performance of polyethylene pipes is one of the hot topics in the field of polymer materials research. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a polyethylene pipe for water supply and a preparation method thereof, which can solve the deficiencies of the prior art and improve the impact strength of the polyethylene pipe.

[0004] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows.

[0005] A method for preparing a polyethylene pipe for water supply comprises the following steps:

[0006] A. Prepare the raw materials. The raw materials include:

[0007] 200 parts of polyethylene,

[0008] 3-5 parts of carbon black masterbatch,

[0009] 1-2 parts of antioxidant,

[0010] 1-2 parts of flame retardant,

[0011] Polypropylene 15 parts;

[0012] B. Put polyethylene and polypropylene into an open mill, heat and mix, let stand and cool for later use;

[0013] C. Put the polyethylene and polypropylene mixture treated in step B, the carbon black masterbatch, the antioxidant and the flame retardant into a feeder for mixing;

[0014] D. Input the mixed raw materials into the extruder for extrusion molding.

[0015] Preferably, the carbon black content of the carbon black masterbatch is 35 wt%.

[0016] Preferably, the antioxidant is 6-di-tert-butyl-p-cresol.

[0017] Preferably, the flame retardant is ammonium polyphosphate.

[0018] Preferably, in step B, the heating temperature is 130-150° C. and the heating time is 3-6 hours.

[0019] Preferably, in step B, the heating temperature is 145° C. and the heating time is 5 h.

[0020] Preferably, in step C, the heating temperature is 180° C. and the heating time is 1 h.

[0021] Preferably, in step D, the head temperature of the extruder is 210°C.

[0022] A polyethylene pipe for water supply is prepared using the method for preparing the polyethylene pipe for water supply.

[0023] The beneficial effect brought about by adopting the above technical solution is that the inventors have found in their research that by adding a small amount of polypropylene to the polyethylene raw material and then premixing it at low temperature, the impact strength of the manufactured polyethylene pipe can be significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a flow chart of Example 1. DETAILED DESCRIPTION

[0025] Example 1

[0026] A method for preparing a polyethylene pipe for water supply comprises the following steps:

[0027] A. Prepare the raw materials. The raw materials include:

[0028] 200 parts of polyethylene,

[0029] 4 parts of carbon black masterbatch,

[0030] 1 part antioxidant,

[0031] 1 part flame retardant,

[0032] Polypropylene 15 parts;

[0033] B. Put polyethylene and polypropylene into an open mill and heat and mix them at a temperature of 145°C for 5 hours. Let them stand and cool for later use.

[0034] C. Put the polyethylene and polypropylene mixture treated in step B, the carbon black masterbatch, the antioxidant and the flame retardant into a material cutter for mixing; the heating temperature is 180° C. and the heating time is 1 hour;

[0035] D. Input the mixed raw materials into the extruder for extrusion molding. The head temperature of the extruder is 210℃.

[0036] Example 2

[0037] A method for preparing a polyethylene pipe for water supply comprises the following steps:

[0038] A. Prepare the raw materials. The raw materials include:

[0039] 200 parts of polyethylene,

[0040] 3 parts of carbon black masterbatch,

[0041] 1 part antioxidant,

[0042] 2 parts of flame retardant,

[0043] Polypropylene 15 parts;

[0044] B. Put polyethylene and polypropylene into an open mill and heat and mix them at a temperature of 145°C for 5 hours. Let them stand and cool for later use.

[0045] C. Put the polyethylene and polypropylene mixture treated in step B, the carbon black masterbatch, the antioxidant and the flame retardant into a material cutter for mixing; the heating temperature is 180° C. and the heating time is 1 hour;

[0046] D. Input the mixed raw materials into the extruder for extrusion molding. The head temperature of the extruder is 210℃.

[0047] Example 3

[0048] A method for preparing a polyethylene pipe for water supply comprises the following steps:

[0049] A. Prepare the raw materials. The raw materials include:

[0050] 200 parts of polyethylene,

[0051] 5 parts of carbon black masterbatch,

[0052] 2 parts of antioxidants,

[0053] 1 part flame retardant,

[0054] Polypropylene 15 parts;

[0055] B. Put polyethylene and polypropylene into an open mill and heat and mix them at a temperature of 145°C for 5 hours. Let them stand and cool for later use.

[0056] C. Put the polyethylene and polypropylene mixture treated in step B, the carbon black masterbatch, the antioxidant and the flame retardant into a material cutter for mixing; the heating temperature is 180° C. and the heating time is 1 hour;

[0057] D. Input the mixed raw materials into the extruder for extrusion molding. The head temperature of the extruder is 210℃.

[0058] Comparative Example 1

[0059] A method for preparing a polyethylene pipe for water supply comprises the following steps:

[0060] A. Prepare the raw materials. The raw materials include:

[0061] 200 parts of polyethylene,

[0062] 4 parts of carbon black masterbatch,

[0063] 1 part antioxidant,

[0064] 1 part flame retardant,

[0065] Polypropylene 15 parts;

[0066] B. Put the raw materials into the cutting machine and mix them; the heating temperature is 180℃ and the heating time is 1h;

[0067] C. Input the mixed raw materials into the extruder for extrusion molding. The head temperature of the extruder is 210℃.

[0068] Comparative Example 2

[0069] A method for preparing a polyethylene pipe for water supply comprises the following steps:

[0070] A. Prepare the raw materials. The raw materials include:

[0071] 200 parts of polyethylene,

[0072] 4 parts of carbon black masterbatch,

[0073] 1 part antioxidant,

[0074] 1 part flame retardant,

[0075] B. Put polyethylene into an open mill and heat and mix it at a temperature of 145°C for 5 hours, and then cool it down for later use;

[0076] C. Put the polyethylene treated in step B, the carbon black masterbatch, the antioxidant and the flame retardant into a material cutter and mix them; the heating temperature is 180° C. and the heating time is 1 hour;

[0077] D. Input the mixed raw materials into the extruder for extrusion molding. The head temperature of the extruder is 210℃.

[0078] Comparative Example 3

[0079] A method for preparing a polyethylene pipe for water supply comprises the following steps:

[0080] A. Prepare the raw materials. The raw materials include:

[0081] 200 parts of polyethylene,

[0082] 4 parts of carbon black masterbatch,

[0083] 1 part antioxidant,

[0084] 1 part flame retardant,

[0085] Polypropylene 15 parts;

[0086] B. Put polyethylene and polypropylene into an open mill and heat and mix them at a temperature of 120°C for 5 hours. Let them stand and cool for later use.

[0087] C. Put the polyethylene and polypropylene mixture treated in step B, the carbon black masterbatch, the antioxidant and the flame retardant into a material cutter for mixing; the heating temperature is 180° C. and the heating time is 1 hour;

[0088] D. Input the mixed raw materials into the extruder for extrusion molding. The head temperature of the extruder is 210℃.

[0089] Comparative Example 4

[0090] A method for preparing a polyethylene pipe for water supply comprises the following steps:

[0091] A. Prepare the raw materials. The raw materials include:

[0092] 200 parts of polyethylene,

[0093] 4 parts of carbon black masterbatch,

[0094] 1 part antioxidant,

[0095] 1 part flame retardant,

[0096] Polypropylene 15 parts;

[0097] B. Put polyethylene and polypropylene into an open mill and heat and mix them at a temperature of 180°C for 5 hours. Let them stand and cool for later use.

[0098] C. Put the polyethylene and polypropylene mixture treated in step B, the carbon black masterbatch, the antioxidant and the flame retardant into a material cutter for mixing; the heating temperature is 180° C. and the heating time is 1 hour;

[0099] D. Input the mixed raw materials into the extruder for extrusion molding. The head temperature of the extruder is 210℃.

[0100] Comparative Example 5

[0101] A method for preparing a polyethylene pipe for water supply comprises the following steps:

[0102] A. Prepare the raw materials. The raw materials include:

[0103] 200 parts of polyethylene,

[0104] 4 parts of carbon black masterbatch,

[0105] 1 part antioxidant,

[0106] 1 part flame retardant,

[0107] Polypropylene 15 parts;

[0108] B. Put polyethylene and polypropylene into an open mill and heat and mix them at a temperature of 145°C for 1 hour. Let them stand and cool for later use.

[0109] C. Put the polyethylene and polypropylene mixture treated in step B, the carbon black masterbatch, the antioxidant and the flame retardant into a material cutter for mixing; the heating temperature is 180° C. and the heating time is 1 hour;

[0110] D. Input the mixed raw materials into the extruder for extrusion molding. The head temperature of the extruder is 210℃.

[0111] Comparative Example 6

[0112] A method for preparing a polyethylene pipe for water supply comprises the following steps:

[0113] A. Prepare the raw materials. The raw materials include:

[0114] 200 parts of polyethylene,

[0115] 4 parts of carbon black masterbatch,

[0116] 1 part antioxidant,

[0117] 1 part flame retardant,

[0118] Polypropylene 15 parts;

[0119] B. Put polyethylene and polypropylene into an open mill and heat and mix them at a temperature of 145°C for 7 hours. Let them stand and cool for later use.

[0120] C. Put the polyethylene and polypropylene mixture treated in step B, the carbon black masterbatch, the antioxidant and the flame retardant into a material cutter for mixing; the heating temperature is 180° C. and the heating time is 1 hour;

[0121] D. Input the mixed raw materials into the extruder for extrusion molding. The head temperature of the extruder is 210℃.

[0122] The impact strength of the polyethylene pipes prepared using the above examples and comparative examples is shown in the following table (tested according to GB / T14152-2001 standard):

[0123]

[0124] It can be seen that the three embodiments of the present invention all have relatively excellent impact resistance.

[0125] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a polyethylene pipe for water supply, characterized in that The following steps are involved: A. Prepare raw materials. The raw materials include: 200 parts of polyethylene, 3-5 parts of carbon black masterbatch, 1-2 parts of antioxidant, 1-2 parts of flame retardant, Polypropylene 15 parts; B. Put polyethylene and polypropylene into an open mill, heat and mix, let stand and cool for later use; the heating temperature is 145°C and the heating time is 5h; C. Put the polyethylene and polypropylene mixture treated in step B, the carbon black masterbatch, the antioxidant and the flame retardant into a feeder and mix them; D. Input the mixed raw materials into the extruder for extrusion molding.

2. The method for preparing a polyethylene pipe for water supply according to claim 1, characterized in that: The carbon black content of the carbon black masterbatch is 35 wt%.

3. The method for preparing a polyethylene pipe for water supply according to claim 1, characterized in that: The antioxidant is 6-di-tert-butyl-p-cresol.

4. The method for preparing a polyethylene pipe for water supply according to claim 1, characterized in that: The flame retardant is ammonium polyphosphate.

5. The method for preparing a polyethylene pipe for water supply according to claim 1, characterized in that: In step C, the heating temperature is 180° C. and the heating time is 1 h.

6. The method for preparing a polyethylene pipe for water supply according to claim 1, characterized in that: In step D, the head temperature of the extruder was 210°C.

Citation Information

Cited By