EVA hot melt adhesive film for sole lamination, preparation method thereof and composite sole obtained therefrom

By using a combination of ethylene-vinyl acetate copolymer with a specific VA content, a vapor-phase silica and a tackifying resin in the hot melt adhesive film, the problem of insufficient bonding strength in the prior art at high temperature is solved, and rubber is realized The high fit fastness and peel strength of the outsole and EVA foamed midsole are suitable for composite shoe materials in high temperature environments.

CN116285764BActive Publication Date: 2024-11-22江苏和和新材料股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211615438.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-15
Publication Date
2024-11-22
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

The prior art is difficult to maintain the bonding strength between the rubber outsole and the EVA foamed midsole under high temperature conditions, resulting in footwear products being degusted in high-temperature environments such as ocean transportation and cannot be used.

Method used

The ethylene-vinyl acetate copolymer with a specific VA content is used as the substrate, and the vapor-phase silica and tackifying resin with a specific specific surface area are combined to significantly improve the interface bonding strength of the hot melt adhesive film to the substrate through synergistic effects. The bonding strength is maintained especially at 80-90°C.

Benefits of technology

Achieves high fit fastness and peel strength between rubber outsoles and EVA foamed midsoles, and is suitable for high-temperature environments, such as container environments for desert and ocean transportation, ensuring that composite shoe materials can maintain excellent bonding performance at high temperatures. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004000240760000031
    Figure BDA0004000240760000031
  • Figure BDA0004000240760000051
    Figure BDA0004000240760000051
  • Figure BDA0004000240760000052
    Figure BDA0004000240760000052
Patent Text Reader

Abstract

The invention discloses an EVA hot-melt adhesive film for sole lamination, a preparation method thereof and a prepared composite sole. The EVA hot-melt adhesive film comprises the following raw materials by weight: 50 to 85 parts of ethylene-vinyl acetate copolymer; 3 to 60 parts of tackifying resin; 0.05 to 10 parts of fumed silica; 0.01 to 2 parts of an antioxidant; in the ethylene-vinyl acetate copolymer, the weight percentage content of the vinyl acetate group is 10 to 50%; the tackifying resin is selected from a combination of at least one of terpene resin, terpene phenol resin and C9 petroleum resin and C5 petroleum resin; the specific surface area of ​​the fumed silica is 90 to 350 m 2 The EVA hot melt adhesive film disclosed in the present invention can achieve high bonding fastness and high peeling strength between the rubber outsole and the EVA foam midsole, and can still maintain excellent bonding strength at 80-90°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of hot-melt adhesive films, and in particular relates to an EVA hot-melt adhesive film for sole lamination, a preparation method thereof, and a composite sole obtained by the preparation. Background Art

[0002] The rubber / foamed EVA composite sole combines the advantages of rubber's wear resistance, foamed sole's lightness and comfort, and has become the most commonly used sole for sports shoes and casual shoes. At present, the bonding of rubber outsoles and EVA foamed midsoles in the market still mainly adopts traditional processes, namely solvent-based chloroprene adhesives (the solvents are mainly toluene and xylene). From production, use to post-processing, a large amount of VOC will be generated, which poses a serious threat to the health of workers and users at the production site, and also causes serious pollution to the environment. In recent years, foreign countries have increasingly stringent requirements on environmental protection indicators for shoe materials. my country has also formulated the latest mandatory standards for shoe glue, which has strict regulations on VOC volatile solvents such as benzene and toluene. Therefore, the use of environmentally friendly solvent-free hot melt adhesives has become a development trend.

[0003] Ethylene-vinyl acetate copolymer (EVA) is a large class of environmentally friendly solvent-free hot melt adhesives. It is widely used in the field of adhesives due to its low cost and wide applicable temperature range. Since EVA contains both crystalline PE segments and non-crystalline vinyl acetate VA groups, physical properties such as softening point, glass transition temperature, adhesion, etc. can be easily achieved through the VA content. It has the advantages of strong formula applicability and obvious bonding effect on the surface of highly polar substrates. It is widely used in hot melt adhesives and other fields. However, because the main raw materials of shoe rubber outsoles include natural rubber, styrene-butadiene rubber and other materials containing unsaturated double bonds and low surface polarity, it is difficult to achieve a high bonding strength effect simply by bonding with EVA hot melt adhesives. Existing EVA hot melt adhesives used for bonding soles are mostly used by compounding EVA with other raw materials.

[0004] For example, the application publication number CN 103756576 A discloses a hot melt adhesive film for bonding shoe soles and its preparation method. The hot melt adhesive film is composed of the following raw materials in parts by weight: 50-60 parts of ethylene-vinyl acetate, 30-60 parts of modified ethylene-ethyl acrylate, 15-35 parts of styrene-butadiene block copolymer, 5-20 parts of terpene resin, 0.1-0.5 parts of BIPB, and 0.1-0.5 parts of BPO. However, the crosslinking agents BIPB and BPO added in this technical solution are peroxide crosslinking agent components. From a functional point of view, they can improve the strength of the hot melt adhesive film, but at the same time, the melt index will be reduced after crosslinking during the pressing process, which will seriously affect the wetting of the adhesive on the substrate surface, resulting in poor interface bonding strength.

[0005] Another example is the application publication number CN 103756580 A, which discloses a hot melt adhesive film for bonding shoe soles and its preparation method. The hot melt adhesive film includes the following raw materials in mass percentage: EVA 60-80%, petroleum resin 10-35%, paraffin 3-15%, and antioxidant 0.5-2%. However, this technical solution can only meet the requirements of laminating a limited variety of outsole adhesives at room temperature, and has poor applicability to outsole adhesives / EVA foamed midsoles of different rubber formula types. More importantly, it is difficult for this formula product to maintain ideal bonding strength at high temperatures.

[0006] For example, the application publication number CN 104559843 A discloses a hot melt adhesive film for bonding rubber / foamed EVA composite soles and its preparation method, wherein the hot melt adhesive film is made of 60-95 parts of polyethylene-ester copolymer, 5-40 parts of rubber, and 0.1-8 parts of additives in parts by weight. However, the compatibility of rubber and EVA in this technical solution is poor, and it is difficult to maintain an ideal uniform system, and the cohesive strength is uneven, which affects the overall bonding strength.

[0007] In addition, for some special working conditions, such as when footwear products pass through the equator in a container during ocean transportation, the ambient temperature is as high as 60-80°C. If the hot melt adhesive film cannot maintain a high bonding strength, it will lead to debonding, and ultimately make the product unusable. Summary of the invention

[0008] In view of the above-mentioned problems existing in the prior art, the present invention discloses an EVA hot-melt adhesive film for sole bonding. The EVA hot-melt adhesive film can achieve high bonding fastness and high peel strength between the rubber outsole and the EVA foam midsole, and can still maintain excellent bonding strength at 80-90°C, and is particularly suitable for special working conditions under high temperature.

[0009] The specific technical solutions are as follows:

[0010] An EVA hot melt adhesive film for sole lamination comprises the following raw materials in parts by weight:

[0011]

[0012] The number average molecular weight of the ethylene-vinyl acetate copolymer is 3000 to 60000 g / mol;

[0013] In the ethylene-vinyl acetate copolymer, the weight percentage content of vinyl acetate groups is 10 to 50%;

[0014] The tackifying resin is selected from a combination of at least one of terpene resin, terpene phenol resin, C9 petroleum resin and C5 petroleum resin;

[0015] The specific surface area of ​​the fumed silica is 100 to 300 m2 / g.

[0016] The invention discloses an EVA hot melt adhesive film specially used for bonding a rubber outsole and an EVA foam midsole. The film takes EVA with a specific VA content as a substrate, adds fumed silica with a specific specific surface area and a specific tackifying resin, and utilizes the mutual synergy of the three to achieve the purpose of significantly improving the interface bonding strength of the hot melt adhesive to the substrate, especially the bonding strength at 80-90°C.

[0017] For ethylene-vinyl acetate copolymer (EVA) as a substrate, if the vinyl acetate group (VA) content is too low, the adhesive layer has a high body strength after the hot melt adhesive film is bonded to the sole, but the adhesive layer has poor wettability at the bonding interface and poor interface bonding strength. If the VA content is too high, the adhesive layer has a high interface bonding strength with the bonding substrate, but the adhesive layer has poor body strength. Selecting an appropriate VA content is a prerequisite for achieving a higher bonding strength. Preferably, the weight percentage content of the VA group is 15 to 40%.

[0018] The main function of the tackifying resin is to improve the wetting of the bonding interface and the intermolecular force (van der Waals force) on the interface. However, since they are all small molecular weight substances, too much addition will affect the cohesive strength of the adhesive layer, and too little addition will reduce the bonding strength of the hot melt adhesive to the sole interface. Therefore, it is necessary to select a suitable addition amount to achieve the desired bonding strength. Preferably, the addition amount of the tackifying resin is 15 to 25 parts by weight.

[0019] In addition, according to the different rubber components in the rubber outsole, the specific composition of the tackifying resin needs to be adjusted. It has been found through experiments that if the natural rubber content in the rubber outsole is high, the tackifying resin with C5 petroleum resin as the main component can achieve a higher bonding effect; if the styrene-butadiene rubber content in the rubber outsole is high, the tackifying resin with terpene, terpene phenol, and C9 petroleum resin as the main components can achieve a better bonding effect.

[0020] Preferably, the tackifying resin is selected from a combination of at least one of terpene resin, terpene phenol resin, C9 petroleum resin and C5 petroleum resin; if C5 petroleum resin is used as component A and at least one of terpene resin, terpene phenol resin, C9 petroleum resin is used as component B, it is further preferred that the mass ratio of component A to component B is 1:1 to 9.

[0021] Fumed silica is a nanometer-sized white powder generated by high-temperature hydrolysis of silicon halides in a hydrogen-oxygen flame, commonly known as fumed silica. In the present invention, fumed silica is used for the first time to prepare an EVA hot-melt adhesive film specifically used for sole bonding. Experiments have shown that, under the premise of selecting a suitable VA content to achieve a higher bonding strength, fumed silica with a specific specific surface area and a specific tackifying resin are added to work together to achieve the purpose of significantly improving the interfacial bonding strength of the hot melt adhesive to the substrate, especially the bonding strength at 80 to 90°C. Preferably, the specific surface area of ​​the fumed silica is 90 to 350 m 2 / g. The use of hydrophobic fumed silica can achieve a better dispersion effect, thereby significantly improving the bonding strength.

[0022] Among the raw materials, the antioxidant is selected from the common antioxidant types in the art, including antioxidant 1010, antioxidant 1076, antioxidant 168, etc., and can be used alone or in combination.

[0023] Other processing aids, such as lubricants, flame retardants, antibacterial agents, desiccants, etc., can be selectively added to the raw materials according to specific usage requirements.

[0024] Other processing aids can be selected from common types in the field. Taking lubricants as an example, they can be selected from common types such as oleamide, erucamide, ethylene bisstearamide, stearic acid, polyethylene wax, polypropylene wax, calcium carbonate, talc, etc., and can be used alone or in combination.

[0025] Based on the above raw material types, preferred are:

[0026] In the EVA, the weight percentage content of VA groups is 15-40%;

[0027] The specific surface area of ​​the fumed silica is 100 to 300 m 2 / g;

[0028] The tackifying resin is selected from a combination of at least one of terpene resin and terpene phenol resin and C5 petroleum resin; the mass ratio of the C5 petroleum resin to the terpene phenol resin and / or the terpene resin is 1:1-9.

[0029] Further preferably, the EVA hot melt adhesive film comprises the following raw materials in parts by weight:

[0030]

[0031] The experiment found that when the EVA hot-melt adhesive film prepared by the above-mentioned preferred fumed silica and tackifying resin is used in combination to form a composite sole with a rubber outsole and an EVA foam midsole, the peeling type of the high temperature resistance test is delamination of the sole material (EVA foam midsole / rubber outsole) rather than delamination of the adhesive layer body / adhesive interface, indicating that the EVA hot-melt adhesive film achieves high bonding fastness and high peeling strength.

[0032] More preferably:

[0033] In the ethylene-vinyl acetate copolymer, the weight percentage content of vinyl acetate groups is 28%;

[0034] The tackifying resin is selected from C5 petroleum resin and terpene phenol resin, and the mass ratio of C5 petroleum resin to terpene phenol resin is 1:1-9;

[0035] The specific surface area of ​​the fumed silica is 160 to 200 m 2 / g.

[0036] Further preferably, the raw material composition comprises, by weight:

[0037]

[0038] The experiment found that through further optimization of the raw material types and raw material composition, the EVA hot melt adhesive film prepared achieved excellent bonding fastness with the rubber outsole and the EVA foam midsole after the sole circumference peeling test. All 24 test points met the standards, and the average peel strength at room temperature was as high as 49N / 10mm. The peeling types of the high temperature resistance test were all delamination of the sole material (delamination of the rubber sole), indicating that it still has excellent bonding fastness and peeling strength at high temperatures (95°C).

[0039] The present invention also discloses a method for preparing the EVA hot melt adhesive film for sole lamination, comprising the following steps:

[0040] The first step: mix the raw materials evenly according to the proportion to obtain a mixture;

[0041] Step 2: Extruding and granulating the mixed material, and drying it to obtain hot melt adhesive particles;

[0042] Step 3: The hot melt adhesive particles are made into an adhesive film with a thickness of 0.03 to 0.3 mm through a casting / blowing film process.

[0043] In step 2, a twin-screw extruder is used for extrusion granulation, and the barrel temperature of the twin-screw extruder is set to 130-150°C.

[0044] The present invention also discloses a composite sole, comprising a rubber outsole, an EVA foam midsole and an EVA hot melt adhesive film for bonding the rubber outsole and the EVA foam midsole. The EVA hot melt adhesive film adopts the EVA hot melt adhesive film for sole bonding disclosed in the present invention.

[0045] Preferably, the raw material components of the rubber outsole include natural rubber and styrene-butadiene rubber;

[0046] The weight ratio of the natural rubber to the styrene-butadiene rubber is 1:1-3.

[0047] Further preferred:

[0048] When the weight ratio of the natural rubber to the styrene-butadiene rubber is 1:1, in the raw material formula of the EVA hot melt adhesive film, the weight percentage content of the vinyl acetate group in the ethylene-vinyl acetate copolymer is 28%; the tackifying resin is selected from C5 petroleum resin and terpene phenol resin, and the mass ratio of C5 petroleum resin to terpene phenol resin is 1:1; the specific surface area of ​​the fumed silica is 160 to 200 m 2 / g.

[0049] When the weight ratio of the natural rubber to the styrene-butadiene rubber is 1:3, in the raw material formula of the EVA hot melt adhesive film, the weight percentage content of the vinyl acetate group in the ethylene-vinyl acetate copolymer is 28%; the tackifying resin is selected from C5 petroleum resin and terpene phenol resin, and the mass ratio of C5 petroleum resin to terpene phenol resin is 1:9; the specific surface area of ​​the fumed silica is 160 to 200 m 2 / g.

[0050] It was found through experiments that under the above-mentioned process parameters, the composite sole prepared can maintain the best bonding strength at 80-90°C.

[0051] Compared with the prior art, the present invention has the following beneficial effects:

[0052] The invention discloses an EVA hot melt adhesive film specially used for bonding a rubber outsole and an EVA foam midsole. The film takes EVA with a specific VA content as a substrate, adds fumed silica with a specific specific surface area and a specific tackifying resin, and utilizes the mutual synergy of the three to achieve the purpose of significantly improving the interface bonding strength of the hot melt adhesive to the substrate, especially the bonding strength at 80-90°C.

[0053] By using the above-mentioned EVA hot melt adhesive film, a higher bonding strength can be achieved between the rubber outsole and the EVA foam midsole, and a high peeling strength can be prepared, which is particularly suitable for composite shoe materials under special working conditions such as desert environments and high-temperature container environments for ocean transportation. DETAILED DESCRIPTION

[0054] The present invention is further described in detail below in conjunction with examples and comparative examples, but the embodiments of the present invention are not limited thereto.

[0055] Example 1

[0056] Step 1: uniformly mix the raw materials according to the weight parts in Table 1 to obtain a mixture;

[0057] Step 2: Add the mixed material into a twin-screw extruder for extrusion, granulation and drying (the barrel temperature is set at 130-150°C) to obtain hot melt rubber particles;

[0058] Step 3: The hot melt adhesive pellets are made into an adhesive film with a thickness of 0.1 mm by a casting / blowing process. The obtained product is the product of Example 1.

[0059] Table 1

[0060]

[0061]

[0062] Example 2

[0063] The preparation process is the same as in Example 1, and the raw materials are mixed evenly according to the weight proportions in Table 2 below.

[0064] Table 2

[0065]

[0066] Example 3

[0067] The preparation process is the same as in Example 1, and the raw materials are mixed evenly according to the weight proportions in Table 3 below.

[0068] Table 3

[0069]

[0070]

[0071] Example 4

[0072] The preparation process is the same as in Example 1, and the raw materials are mixed evenly according to the weight proportions in Table 4 below.

[0073] Table 4

[0074]

[0075] Example 5

[0076] The preparation process is the same as in Example 1, and the raw materials are mixed evenly according to the weight proportions in Table 5 below.

[0077] Table 5

[0078]

[0079]

[0080] Example 6

[0081] The preparation process is the same as in Example 1, and the raw materials are mixed evenly according to the weight proportions in Table 6 below.

[0082] Table 6

[0083]

[0084] Example 7

[0085] The preparation process is the same as in Example 1, and the raw materials are mixed evenly according to the weight proportions in Table 7 below.

[0086] Table 7

[0087]

[0088]

[0089] Example 8

[0090] The preparation process is the same as in Example 1, and the raw materials are mixed evenly according to the weight proportions in Table 8 below.

[0091] Table 8

[0092]

[0093] Example 9

[0094] The preparation process is the same as in Example 1, and the raw materials are mixed evenly according to the weight proportions in Table 9 below.

[0095] Table 9

[0096]

[0097]

[0098] Comparative Example 1

[0099] The preparation process was the same as in Example 1, and Japanese Sumitomo KA-10 (VA content 28 wt.%) was selected as the substrate, but no fumed silica was added to the raw materials, and the raw materials were mixed evenly according to the weight proportions shown in Table 10 below.

[0100] Table 10

[0101]

[0102] Comparative Example 2

[0103] The preparation process was the same as in Example 1, and Japanese Sumitomo KA-10 (VA content 28 wt.%) was selected as the base material, but no tackifying resin was added to the raw materials, and the raw materials were mixed evenly according to the weight proportions shown in Table 11 below.

[0104] Table 11

[0105]

[0106]

[0107] Comparative Example 3

[0108] The preparation process is the same as in Example 1, and the raw materials are mixed evenly according to the weight proportions in Table 12 below.

[0109] Table 12

[0110]

[0111] Comparative Example 4

[0112] The preparation process is the same as in Example 1, but ordinary silicon dioxide is selected instead of fumed silicon dioxide, and the raw materials are mixed evenly according to the weight proportions in Table 13 below.

[0113] Table 13

[0114]

[0115]

[0116] Performance Testing:

[0117] 1. Sole circumference peeling test method

[0118] Test purpose: Test the adhesion between the outsole and midsole;

[0119] Test scope: for composite soles with rubber outsole / EVA foam midsole structure laminated with EVA hot melt adhesive film;

[0120] Testing equipment: tensile machine, ruler, knife;

[0121] Test conditions: room temperature (25±2℃);

[0122] Test material: composite sole

[0123] Parameter requirements:

[0124] 1. Cutting test section width: 10±1mm;

[0125] 2.Tensile testing machine test speed: 200mm / min.

[0126] Test steps:

[0127] 1) The sample is placed at room temperature for more than 24 hours;

[0128] 2) Draw a line 10 mm away from the edge of the sole sample (make sure the line is 10 mm away from the edge of the sample);

[0129] 3) Use a knife to carve along the drawn line, making sure the cut is deep enough (penetrating the rubber bottom to the bottom layer of the EVA foam);

[0130] 4) Use a marker pen to evenly mark points on the cut sample, one point every 20 mm, for a total of 24 test points;

[0131] 5) Use a knife to cut a 10mm wide and 20mm long cut along the edge of the sole where the outsole / midsole meet, clamp the sample on the tensile testing machine, and set the tensile testing machine speed to 200mm / min;

[0132] 6) Start the test and record the minimum value between every two points;

[0133] 7) If you encounter unsatisfactory points, please note the type of delamination (interface delamination / adhesive body delamination / sole material delamination).

[0134] Note:

[0135] ①Pull in clockwise direction;

[0136] ②The peel strength values ​​at all points must be greater than the standard value (30N / 10mm) to be qualified.

[0137] 2. High temperature resistance test method for rubber outsole / EVA foam midsole:

[0138] Draw two parallel straight lines in the middle area of ​​the sole (extending from the toe to the heel) with an interval of 10 mm, and use a knife to cut vertically along the drawn lines, ensuring that the knife cut line is deep enough (penetrating the rubber outsole and cutting into the EVA foam midsole). Put the shoes into an oven (the oven temperature is set to 95°C), take them out after baking for 30 minutes, and use pliers to peel off the cut part while it is still hot (10 mm long strips), observe the peeling type of the midsole and the outsole (interface delamination / adhesive layer body delamination / sole material delamination), and record the results in Table 14.

[0139] Table 14

[0140]

[0141]

Claims

1. A composite sole, comprising a rubber outsole, an EVA foam midsole and an EVA hot melt adhesive film for bonding the rubber outsole and the EVA foam midsole, characterized in that: The EVA hot melt adhesive film comprises the following raw materials in parts by weight: 50-85 parts of ethylene-vinyl acetate copolymer; 3-60 parts of tackifying resin; 0.05-10 parts of fumed silica; Antioxidant 0.01~2 parts; The number average molecular weight of the ethylene-vinyl acetate copolymer is 3000-60000 g / mol; In the ethylene-vinyl acetate copolymer, the weight percentage content of vinyl acetate groups is 28%; The tackifying resin is selected from C5 petroleum resin and terpene phenol resin, and the mass ratio of C5 petroleum resin to terpene phenol resin is 1:1-9; The specific surface area of ​​the fumed silica is 160-200 m 2 / g.

2. The composite sole according to claim 1, characterized in that: By weight, it includes the following raw materials: 70-80 parts of ethylene-vinyl acetate copolymer; 15-25 parts of tackifying resin; 1-5 parts of fumed silica; Antioxidant 0.01~2 parts; 1~3 parts of lubricant.

3. The composite sole according to claim 1, characterized in that: By weight, it includes the following raw materials: 73-80 parts of ethylene-vinyl acetate copolymer; 20 parts of tackifying resin; 3-5 parts of fumed silica; Antioxidant 0.01~2 parts; 1~3 parts of lubricant.

4. The composite sole according to claim 1, characterized in that: The preparation method of the EVA hot melt adhesive film for sole bonding comprises the following steps: The first step: mix the raw materials evenly according to the proportion to obtain a mixture; Step 2: Extruding and granulating the mixed material, and drying it to obtain hot melt adhesive particles; Step 3: The hot melt adhesive particles are made into an adhesive film with a thickness of 0.03-0.3 mm through a casting / blowing film process.

5. The composite sole according to claim 1, characterized in that: The raw material components of the rubber outsole include natural rubber and styrene-butadiene rubber; The weight ratio of the natural rubber to the styrene-butadiene rubber is 1:1-3.