A die-casting aluminum silicon alloy and a die-casting method for refining pre-crystallization structure

By introducing specific elements into die-cast aluminum-silicon alloys to refine the structure, the problem of poor mechanical properties of aluminum-silicon alloys in the prior art is solved, the formation of high-iron content and uniform structure is achieved, and the mechanical properties of aluminum alloys are significantly improved.

CN116287883BActive Publication Date: 2024-11-01CHINA FAW CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310158894.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-24
Publication Date
2024-11-01
Estimated Expiration
2043-02-24

AI Technical Summary

Technical Problem

The existing die-cast aluminum-silicon alloys have shortcomings in mechanical properties, mainly due to gas retention and tissue unevenness caused by high-speed liquid flow filling, as well as stress concentration caused by thick needle-shaped iron-rich phase formed by iron elements. Reduces the mechanical properties of the material.

Method used

By introducing Mn, Mo, V and other elements into die-cast aluminum-silicon alloys, refining the primary iron-rich phase, increasing elements such as Nb, Zr, Ti, B, and Ni to refine the α-Al grains, forming sub-eutectic aluminum with high iron content Silicon alloy, high-pressure vacuum die-casting process is used to reduce the size and distribution unevenness of precrystallized structure.

Benefits of technology

It significantly improves the mechanical properties of die-cast aluminum alloy, including improving the content and distribution uniformity of iron elements, reducing shrinkage defects, and enhancing the tensile strength and elongation of the castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116287883B_ABST
    Figure CN116287883B_ABST
Patent Text Reader

Abstract

A die-cast aluminum silicon alloy and a die-casting method for refining pre-crystallization structure, which relates to the technical field of aluminum silicon alloy materials, solves the problem of poor mechanical properties of die-cast aluminum silicon alloys, and can be applied to the manufacture of automobiles, high-speed trains and large aircraft. The alloy contains 8-11wt% silicon, 0.3-0.8wt% iron, 0.2-0.6wt% manganese, 0.1-0.5wt% molybdenum, 0.1-0.5wt% vanadium, 0.1-0.5wt% zirconium, 0.01-0.5wt% niobium, 0.1-0.5wt% titanium, 0.01-0.3wt% boron, 0.01-0.2wt% nickel, 0.02-0.1wt% strontium, no more than 0.1wt% impurities and the remainder aluminum. The alloy ingot is placed in a heat preservation furnace for melting and then heat preservation, argon gas is introduced and stirred; the aluminum liquid is subjected to slag treatment to remove surface scum; the aluminum liquid is allowed to stand, and the temperature is reduced to a specific temperature before high-pressure die casting, and a vacuum machine is used for vacuuming.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum-silicon alloy materials, and in particular to a die-casting aluminum-silicon alloy and a die-casting method for refining a pre-crystallization structure. Background Art

[0002] Due to the need for energy conservation and emission reduction, automobile lightweighting technology has become the main trend of the development of the world's automobile industry. By reducing the weight of the entire vehicle, the energy consumption of the vehicle can be effectively reduced and CO2 emissions can be reduced. The use of lightweight materials is the most effective way to achieve automobile lightweighting.

[0003] Aluminum-silicon alloy has a low density, only 1 / 3 of that of steel, and high specific strength, making it the most widely used lightweight material. Cast aluminum alloy is most widely used in the production of automotive parts, such as engines, car wheels, etc. However, due to the limitations of its mechanical properties, the application of cast aluminum-silicon alloy has been restricted.

[0004] As a casting process with high production efficiency, high product dimensional accuracy and no need for subsequent processing, the die-casting process has been widely used in the manufacture of automotive parts. However, during the die-casting process, due to the high-speed filling of the liquid flow, the gas entrained by the melt cannot be discharged, and remains inside the casting to form holes, which reduces the mechanical properties of the die-casting; at the same time, due to the high cooling rate of the die-casting process, the core of the die-casting structure surface is uneven. The pre-crystallized structure formed in the pressure chamber is large in size and easily gathers in the core of the die-casting, causing shrinkage defects, which is easy to produce stress concentration when subjected to force, reducing the mechanical properties of the die-casting. Therefore, it is extremely important to refine the pressure chamber pre-crystallized structure in the die-casting aluminum-silicon alloy to improve the mechanical properties of the die-casting.

[0005] Iron is one of the main impurity elements in aluminum silicon alloys. It is inevitable in aluminum melts, and it is difficult and costly to remove. The iron element in aluminum melts easily forms a coarse needle-shaped iron-rich phase with aluminum and silicon elements, which can easily cause stress concentration under stress, split the matrix, and reduce the mechanical properties. Studies have shown that the increase of trace iron elements will lead to a sharp drop in the elongation of castings. However, in die-cast aluminum silicon alloys, a certain content of iron elements can ensure the demoulding properties of castings and reduce the cost of controlling the iron content in aluminum melts during production. Therefore, it is very necessary to develop die-cast aluminum silicon alloys with high iron content for production.

[0006] In conventional die-cast aluminum-silicon alloys, the morphology of the iron-rich phase is usually regulated by controlling the iron-manganese ratio. Under the appropriate iron-manganese ratio, the aspect ratio of the needle-shaped iron-rich phase decreases and is completely transformed into a blocky iron-rich phase. However, the coarse blocky iron-rich phase formed in the die-casting chamber still exists and is a brittle phase, which seriously affects the mechanical properties of the material. It is easy to concentrate stress during the stretching process, induce cracks and expand, and eventually lead to the fracture of the casting. Summary of the invention

[0007] In order to solve the problem of poor mechanical properties of existing die-cast aluminum-silicon alloys, the present invention provides a die-casting aluminum-silicon alloy and a die-casting method for refining a pre-crystallization structure.

[0008] The technical solution of the present invention is as follows:

[0009] A die-cast aluminum-silicon alloy comprises 8-11wt% silicon, 0.3-0.8wt% iron, 0.2-0.6wt% manganese, 0.1-0.5wt% molybdenum, 0.1-0.5wt% vanadium, 0.1-0.5wt% zirconium, 0.01-0.5wt% niobium, 0.1-0.5wt% titanium, 0.01-0.3wt% boron, 0.01-0.2wt% nickel, 0.02-0.1wt% strontium, no more than 0.1wt% impurities and the balance aluminum.

[0010] Preferably, under vacuum, the yield strength of the die-cast alloy rod sample is 150-170 MPa, the tensile strength is 290-300 MPa, and the elongation is 10-16%.

[0011] Preferably, the raw materials are pure aluminum, crystalline silicon, aluminum-iron alloy, aluminum-manganese alloy, aluminum-molybdenum alloy, aluminum-vanadium alloy, aluminum-zirconium alloy, aluminum-titanium alloy, aluminum-niobium alloy, aluminum-boron alloy, aluminum-nickel alloy and aluminum-strontium alloy and are smelted to obtain the alloy.

[0012] A die-casting method for refining a pre-crystallized structure, using the die-casting aluminum-silicon alloy as described above, the method specifically comprises the following steps:

[0013] S1, placing the die-cast aluminum-silicon alloy ingot into a holding furnace, melting it, and then keeping it warm, introducing argon gas and stirring it with a stirrer;

[0014] S2, performing slag removal on the surface of the aluminum liquid after stirring;

[0015] S3. Let the aluminum liquid stand until the temperature drops to a certain level, then perform high pressure die casting and use a vacuum machine to evacuate the liquid.

[0016] Preferably, the temperature of the insulation furnace in step S1 is 710°C.

[0017] Preferably, the insulation time in step S1 is 30 minutes.

[0018] Preferably, the stirring time in step S1 is 20 min.

[0019] Preferably, the specific temperature in step S3 is 695°C.

[0020] Preferably, the process parameters of the high pressure die casting are as follows:

[0021] The pouring temperature is 695°C, the mold temperature is 150°C, the mold gate ratio is 30:1, the low speed is 0.1-0.2m / s, and the high speed is 2.75m / s.

[0022] An application of the die-cast aluminum silicon alloy as described above in the fields of automobile, high-speed train and large aircraft manufacturing.

[0023] Compared with the prior art, the present invention solves the problem of poor mechanical properties of the existing die-cast aluminum silicon alloy, and the specific beneficial effects are:

[0024] The present invention introduces Mn, Mo and V elements to refine the primary iron-rich phase in the die-casting structure, introduces Nb, Zr, Ti, B, V and Ni elements to refine the primary α-Al grains in the structure, increases heterogeneous nucleation points, promotes nucleation, and reduces the size of the primary α-Al in the pressure chamber, and finally develops a die-cast hypoeutectic aluminum-silicon alloy with a high iron content; the high-strength and toughness die-casting aluminum-silicon alloy has a high iron content, and the high iron content is conducive to demoulding and reduces costs, and effectively reduces the size of the primary iron-rich phase and the primary α-Al grains in the pre-crystallization structure of the pressure chamber, thereby greatly improving the mechanical properties of the die-casting aluminum alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a primary iron-rich phase and primary α-Al structure diagram of AlSi10MnMg alloy in a specific implementation manner;

[0026] Figure 2 The primary iron-rich phase and primary α-Al structure diagram of the die-cast aluminum-silicon alloy prepared in a specific embodiment;

[0027] Figure 3 It is a diagram of the tensile mechanical properties of the AlSi10MnMg alloy and the prepared die-cast aluminum silicon alloy in a specific implementation manner. DETAILED DESCRIPTION

[0028] In order to make the technical solution of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the specification of the present invention. It should be noted that the following embodiments are only used to better understand the technical solution of the present invention and should not be understood as a limitation to the present invention.

[0029] In this embodiment, pure aluminum, crystalline silicon, aluminum-iron alloy, aluminum-manganese alloy, aluminum-molybdenum alloy, aluminum-vanadium alloy, aluminum-zirconium alloy, aluminum-titanium alloy, aluminum-niobium alloy, aluminum-boron alloy, aluminum-nickel alloy and aluminum-strontium alloy are used as raw materials for smelting to obtain a die-cast aluminum-silicon alloy ingot. The composition of the obtained die-cast aluminum-silicon alloy ingot is as follows: Si: 9.42wt%; Fe: 0.43wt%; Mo: 0.1wt%; Mn: 0.33wt%; V: 0.1wt%; Zr: 0.23wt%; Ti: 0.1wt%; Nb: 0.01wt%; B: 0.01wt%; Ni: 0.01wt%; Sr: 0.023wt%; the remainder is Al.

[0030] The die-cast aluminum silicon alloy ingot is placed in a heat preservation furnace for melting and heat preservation, and argon gas is introduced and stirred with a stirrer; the stirred aluminum liquid is subjected to slag treatment to remove the scum on the surface of the aluminum liquid; the aluminum liquid is allowed to stand, and after the temperature drops to a specific temperature, high-pressure die casting is performed. The die casting process is as follows: pouring temperature 695°C, mold temperature 150°C, mold gate ratio 30:1, low speed 0.1-0.2m / s, high speed 2.75m / s. A Toyo vacuum machine is used for vacuuming. Under vacuum conditions, the effective vacuum degree of the cavity set by the die casting machine is less than 8KPa.

[0031] A commercial die-cast aluminum silicon AlSi10MnMg alloy was used as a comparison, and its composition was: Si: 10.14wt%; Fe: 0.11wt%; Mn: 0.64wt%; Mg: 0.31wt%; Ti: 0.07wt%; Sr: 0.025wt%; and the balance was Al.

[0032] The prepared die-cast aluminum silicon alloy and die-cast aluminum silicon AlSi10MnMg alloy were tested for their microstructure and mechanical properties, and the test results are shown in the attached figures. Figure 1 This is the microstructure of the primary iron-rich phase and primary α-Al in the pressure chamber of the AlSi10MnMg alloy. Figure 2This is the microstructure diagram of the primary iron-rich phase and primary α-Al in the pressure chamber of the prepared die-cast aluminum-silicon alloy. By comparison, it can be seen that the iron-rich phase in the AlSi10MnMg alloy is in the form of coarse blocks with a size of about 10 μm; after adding Mo and V elements to the die-cast aluminum silicon alloy prepared in this embodiment, the size of the iron-rich phase is greatly reduced to about 1 μm, and the content of large-sized iron-rich phase is small; the primary α-Al grain size in the AlSi10MnMg alloy is coarse and has a higher degree of dendrite formation. After statistics, the average size is about 40 μm; after adding trace elements such as Nb, Zr, Ti, V, B and Ni to the die-cast aluminum silicon alloy prepared in this embodiment, the size of the primary α-Al grains is greatly reduced due to the generation of second phase particles, such as Al3Nb, Al3Zr, Al3Ti, Al3Ni, VB2, TiB2 and NbB2, which promote heterogeneous nucleation, and the average size is about 20 μm after statistics, and it is more evenly distributed in the organization. Figure 3 This is a tensile mechanical property diagram of the AlSi10MnMg alloy in Example 1 and the die-cast aluminum silicon alloy prepared in this example. Compared with the AlSi10MnMg alloy, the die-cast aluminum silicon alloy prepared in this example maintains tensile strength and yield strength under high iron content conditions, and the elongation is significantly improved, showing better mechanical properties.

[0033] Although specific embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, substitute and vary the above embodiments within the scope of the present invention.

Claims

1. A die-cast aluminum silicon alloy, It is characterized in that Containing 8-11wt% silicon, 0.3-0.8wt% iron, 0.2-0.6wt% manganese, 0.1-0.5wt% molybdenum, 0.1-0.5wt% vanadium, 0.1-0.5wt% zirconium, 0.01-0.5wt% niobium, 0.1-0.5wt% titanium, 0.01-0.3wt% boron, 0.01-0.2wt% nickel, 0.02-0.1wt% strontium, no more than 0.1wt% impurities and the balance aluminum; The yield strength of the die-cast alloy rod sample is 150-170 MPa, the tensile strength is 290-300 MPa, and the elongation is 10-16%.

2. A die-casting method for refining pre-crystallized structure, It is characterized in that Using the die-cast aluminum-silicon alloy as claimed in claim 1, the method specifically comprises the following steps: S1, placing the die-cast aluminum-silicon alloy ingot into a holding furnace, melting it, and then keeping it warm, introducing argon gas and stirring it with a stirrer; The die-cast aluminum-silicon alloy ingot is prepared by smelting pure aluminum, crystalline silicon, aluminum-iron alloy, aluminum-manganese alloy, aluminum-molybdenum alloy, aluminum-vanadium alloy, aluminum-zirconium alloy, aluminum-titanium alloy, aluminum-niobium alloy, aluminum-boron alloy, aluminum-nickel alloy and aluminum-strontium alloy as raw materials; S2, performing slag removal on the surface of the aluminum liquid after stirring; S3. Let the aluminum liquid stand until the temperature drops to a specific temperature, then carry out high-pressure die casting. Use a vacuum machine to evacuate the air. Under vacuum conditions, the effective vacuum degree of the cavity set by the die-casting machine is lower than 10KPa.

3. The die-casting method for refining the pre-crystallization structure according to claim 2, It is characterized in that The temperature of the holding furnace in step S1 is 710°C.

4. The die-casting method for refining the pre-crystallization structure according to claim 2, It is characterized in that The insulation time in step S1 is 30 minutes.

5. The die-casting method for refining the pre-crystallization structure according to claim 2, It is characterized in that The stirring time in step S1 is 20 min.

6. The die-casting method for refining the pre-crystallization structure according to claim 2, It is characterized in that The specific temperature in step S3 is 695°C.

7. The die-casting method for refining the pre-crystallization structure according to claim 2, It is characterized in that The process parameters of the high pressure die casting are as follows: The pouring temperature is 695°C, the mold temperature is 150°C, the mold gate ratio is 30:1, the low speed is 0.1-0.2m / s, and the high speed is 2.75m / s.

8. Application of the die-cast aluminum-silicon alloy as claimed in claim 1 in the fields of automobile, high-speed train and large aircraft manufacturing.