A 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance and a production method thereof
Through austenite zone rolling and online rapid quenching process, combined with deep degassing and vacuum treatment, the problems of long production cycle and high cost of steel plates in the existing technology were solved, and 1100MPa grade rare earth wide-thick steel plates were prepared, with high strength and resistance Wear and corrosion resistance, suitable for industrial machinery and equipment under severe working conditions.
Patent Information
- Application Number
- CN202310054977.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-03
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-02-03
AI Technical Summary
When preparing high-strength, wear-resistant and corrosion-resistant wide-thick steel plates, the production cycle is long, the manufacturing cost is high, and there is no requirement for corrosion resistance index, making it difficult to meet the service needs of industrial machinery and equipment under strict working conditions.
The austenite zone rolling and online rapid quenching process were adopted, and the 1100MPa grade rare earth wide-thick steel plate was prepared through KR desulfurization pretreatment, LF ladle refining furnace, RH deep degassing process and vacuum treatment, combined with straight arc continuous casting and dynamic cooling technology. , simplifies the heat treatment steps and reduces production cycle and costs.
It has achieved high strength, low cost, corrosion resistance, easy welding and low temperature toughness of 1100MPa grade steel plate, which has improved the wear and corrosion resistance of the steel plate, and has good processing performance, meeting the application needs under strict working conditions.
Smart Images

Figure CN116287979B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a 1100MPa-grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance and a production method thereof, and in particular to a wide and thick plate with severe service conditions of impact resistance, wear resistance and corrosion resistance. Background Art
[0002] In recent years, with the increasing scarcity of mineral resources and the complex conditions of deep underground mining, new high-strength, corrosion-resistant, wear-resistant, and low-cost materials have emerged, which have improved the service life and safety of industrial machinery and equipment and effectively reduced the manufacturing cost of the industrial chain.
[0003] At present, domestic patents and documents on bridge steel of the same level include:
[0004] Chinese patent CN107354382A discloses "wear-resistant thick steel plate with low-temperature toughness and its manufacturing method", the composition mass percentage is: C: more than 0.10 and less than 0.20%, Si: 0.05-0.5%, Mn: 0.5-1.5%, Cr: 0.05-1.20%, Nb: 0.01-0.08%, B: 0.0005-0.003%, Al: 0.01-0.08%, N: 0.0005-0.008%, P: less than 0.05%, S: less than 0.005%, O: less than 0.008%, and V, Ti, Cr, Ni, Cu, Mo and other alloys are selectively added, and the rest is Fe and unavoidable impurities. This patent has no requirements for the corrosion resistance index. It is prepared by rolling, reheating and quenching, with a long production cycle and high manufacturing cost.
[0005] Chinese patent CN 110184532 A invention discloses "a low alloy wear-resistant steel plate with excellent -60℃ ultra-low temperature impact toughness and its manufacturing method", the chemical composition of the steel is C: 0.12~0.20%, Si: 0.10~0.40%, Mn: 0.8~1.30%, Nb: 0.010~0.040%, V: 0.020~0.050%, Ti: ≤0.010%, Al: 0.04~0.08%, Ni: ≤0.1%, Cu: ≤0.1%, Cr: 0.20~0.60%, Mo: 0.30~0.8 0%, B: 0.001~0.005%, Ca: ≤0.0010%, P: ≤0.010%, S: ≤0.0015%, O: ≤0.0015%, N: ≤0.0035%, H: ≤0.0002%, and satisfy 0.15≤(Mn+Mo) / 10+Cr / 20≤0.26, S+P+O+N+H≤0.015%, the balance is Fe and unavoidable impurity elements. This patent has no requirements for the corrosion resistance index. It is prepared by rolling, reheating and quenching, with a long production cycle and high manufacturing cost.
[0006] Chinese patent CN110592491A discloses "a high wear-resistant martensite / austenite dual-phase wear-resistant steel plate and its manufacturing method". The steel contains 0.20% to 0.40% C, 0.05% to 0.60% Si, 3.0% to 6.0% Mn, 0.40% to 0.80% Ti, etc. This patent adopts rolling, reheating and annealing processes, with a long production cycle and high manufacturing cost. Summary of the invention
[0007] The purpose of the present invention is to provide a 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance and a production method thereof. Comprehensive considerations are given to cost design, production cycle, organizational performance control, wear resistance, corrosion resistance, welding and processing performance, and an austenite zone rolling and online rapid quenching process are adopted. No need for heat treatment and reheating before quenching, so as to prepare a 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance. The steel plate has the characteristics of high strength, low cost, corrosion resistance, easy welding, no deformation during processing and high low-temperature toughness.
[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0009] The invention discloses a 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance. The chemical composition thereof is C: 0.11-0.15%, Si: 0.20-0.50%, Mn: 1.00-1.35%, P: 0.02%-0.07%, S≤0.003% by weight, Als: 0.017-0.032%, B: 0.0006-0.0016%, rare earth Re: 0.001-0.02%, Nb, V, Ti, Cr, Mo, Cu, Ni alloy elements are selectively added, 0.010%≥Nb+V+Ti≤0.095%, 0.7%≥Cr+Mo+Cu+Ni≤2.0%, and the balance is Fe and unavoidable impurities.
[0010] Furthermore, its chemical composition by weight percentage is C: 0.15%, Si: 0.20%, Mn: 1.0%, P: 0.020%, S: 0.001%, Als: 0.030%, B: 0.0016%, rare earth Re: 0.001%, Nb: 0.01%, Ti: 0.055%, Cr: 0.4%, Cu: 0.31%, Ni: 0.25%, and the balance is Fe and inevitable impurities.
[0011] Furthermore, its chemical composition by weight percentage is C: 0.14%, Si: 0.25%, Mn: 1.10%, P: 0.025%, S: 0.002%, Als: 0.025%, B: 0.0012%, rare earth Re: 0.012%, Nb: 0.01%, Ti: 0.012%, Cr: 0.5%, Cu: 0.28%, Ni: 0.28%, and the balance is Fe and inevitable impurities.
[0012] Furthermore, its chemical composition by weight percentage is C: 0.11%, Si: 0.40%, Mn: 1.18%, P: 0.060%, S: 0.003%, Als: 0.017%, B: 0.0006%, rare earth Re: 0.015%, Ti: 0.015%, Cr: 0.48%, Cu: 0.25%, Ni: 0.30%, and the balance is Fe and inevitable impurities.
[0013] A method for producing a 1100MPa grade rare earth wide and thick steel plate having both wear resistance and corrosion resistance, characterized by comprising:
[0014] The main steps and process parameters are as follows:
[0015] 1) Smelting
[0016] The molten iron and high-quality scrap steel that have been pre-treated by KR desulfurization are used as raw materials. The bottom blowing of the converter adopts the full-process argon blowing mode, and the end point is hit once to reduce the increase of nitrogen in the molten steel due to supplementary blowing. The LF ladle refining furnace further deoxidizes, desulfurizes, removes inclusions, adjusts the composition and temperature. The argon blowing intensity must be strictly controlled. The argon blowing curve is formulated according to the principle of strong in the early stage, relatively strong in the middle stage, and weak in the late stage. While ensuring deoxidation, deep desulfurization, and alloying, the secondary oxidation and nitrogen increase in the refining process are reduced. The RH process adopts a circulating deep degassing process to greatly reduce the content of gases such as hydrogen, oxygen, and nitrogen while ensuring the stability of the molten steel temperature, reducing the adverse effects of harmful gases on steel quality. The rare earth lanthanum-cerium alloy is added from the vacuum chute 3-5 minutes before the vacuum treatment is completed and re-pressurized to ensure the rare earth recovery rate. The final molten steel smelting composition has the following mass percentages: C: 0.11-0.15%, Si: 0.20-0.50%, Mn: 1.00-1.35%, P: 0.02%-0.08%, S≤0.003%, Als: 0.017-0.032%, B: 0.0006-0.0016%, rare earth Re: 0.001-0.02%, and Nb, V, Ti, Cr, Mo, Cu, and Ni alloy elements are selectively added, 0.010%≥Nb+V+Ti≤0.095%, 0.7%≥Cr+Mo+Cu+Ni≤2.0%, and the balance is Fe and unavoidable impurities.
[0017] 2) Continuous casting
[0018] The continuous casting machine is a straight arc continuous casting machine, which adopts argon blowing protection for large and medium ladle water inlets, dynamic light pressure at the end of solidification, 380A high current electromagnetic stirring and optimized dynamic secondary cooling technology. Through constant temperature and constant pulling speed process (0.9-1.1m / min), taking into account the low superheat casting (25-35℃), the defects such as center segregation, center looseness, cracks, and vibration marks of the continuous casting billet are reduced. Finally, high-quality slabs with a thickness of 250mm and 300mm are produced according to the thickness of the finished product.
[0019] 3) Heating
[0020] The steel slab is heated in the heating furnace to fully ensure the heating temperature and soaking time of the steel slab. The heating temperature is controlled at 1200℃~1250℃, the heating time is controlled at 220-300min, and the holding time is greater than 60min to ensure the full solid solution of the alloy elements and the uniform temperature of the slab.
[0021] 4) High temperature rolling
[0022] The rolling adopts austenite zone rolling, and the deformation of each pass is increased during rough rolling. When the thickness is greater than 30mm, the horizontal rolling + longitudinal rolling method is adopted. The slab length widening is preferred to ensure the reduction rate of the extension pass and improve the uniformity of the transverse and longitudinal organizational properties. The starting rolling temperature is 1190-1250℃, and the relative reduction rate of a single pass is controlled at more than 20% for at least two passes; the deformation of each pass is strictly controlled in the finishing rolling stage, the finishing rolling starting temperature is ≥1050℃, and the starting rolling thickness is set to 2.0-3.5 times the finished product thickness according to the finished product thickness requirements. The rolling speed is 2.0m / s-5.0m / s, and the austenite temperature is calculated according to the composition. The final rolling temperature is 860-930℃, 20℃ above the austenite temperature.
[0023] 5) Rapid cooling
[0024] The steel plate is rapidly cooled after rolling. According to the martensitic transformation temperature and plate shape control, the roller speed, water pressure and water volume are controlled to achieve a surface red-return temperature of 150℃~350℃ after cooling.
[0025] Compared with the prior art, the beneficial technical effects of the present invention are: BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The present invention will be further described below in conjunction with the accompanying drawings.
[0027] Figure 1 The metallographic structure is 200 times that of the steel plate at 1 / 2 thickness in Example 1 of the present invention. DETAILED DESCRIPTION
[0028] The present invention is described in more detail below with examples. Due to the large range of specifications, these examples are only descriptions of typical specifications of the present invention and do not limit the scope of the present invention in any way.
[0029] Example 1
[0030] The raw material molten iron is subjected to deep desulfurization, top and bottom blowing in converter, argon blowing in ladle, LF refining outside furnace, RH vacuum treatment and continuous casting process to obtain 250mm and 300mm thick slabs with chemical composition shown in Table 1. The slab heating temperature is 1210℃, the heating time of 300mm thick slab is 290min, the first stage rolling temperature is 1210℃, the slab length direction is used for widening, the single pass relative reduction rate is controlled at more than 20% for at least two passes, when the thickness of the rolled piece is 80mm (4 times the thickness of the finished product), the second stage finishing rolling is then carried out, the starting rolling temperature is 1080℃, the final rolling temperature is 921℃, and the thickness of the finished steel plate is 20mm; after rolling, the steel plate enters the accelerated cooling equipment, the surface red temperature is 330℃, and the offline stacking is more than 72 hours to obtain 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance.
[0031] Table 1 Chemical composition and corrosion resistance index (wt%) of Examples 1 to 3 of the present invention
[0032] Example C Si Mn Cr Cu Ni Nb Ti P S Als B Re Corrosion resistance I 1 0.15 0.20 1.00 0.4 0.31 0.25 0.01 0.055 0.020 0.001 0.030 0.0016 0.001 6.3 2 0.14 0.25 1.10 0.5 0.28 0.28 0.01 0.012 0.025 0.002 0.025 0.0012 0.012 6.5 3 0.11 0.40 1.30 0.48 0.25 0.3 0.015 0.060 0.003 0.017 0.0006 0.015 7.0
[0033] Example 2
[0034] The smelting and continuous casting implementation methods are the same as those in Example 1. The slab heating temperature is 1210°C, the heating time for the slab with a thickness of 300mm is 290min, the first-stage rolling temperature is 1230°C, and the slab is widened in the length direction. The relative reduction rate of a single pass is controlled at more than 20% for at least two passes. When the thickness of the rolled piece is 100mm (4 times the thickness of the finished product), the second-stage finishing rolling is carried out, with a starting rolling temperature of 1080°C, a final rolling temperature of 899°C, and a finished steel plate thickness of 25mm. After rolling, the steel plate enters an accelerated cooling device, the surface reddening temperature is 267°C, and the steel plate is stacked offline for more than 72 hours to obtain a 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance.
[0035] Example 3
[0036] The smelting and continuous casting implementation methods are the same as those in Example 1. The slab heating temperature is 1210°C, the slab heating time is 290min for a thickness of 300mm, the first-stage rolling temperature is 1210°C, the slab is widened in the length direction, and the relative reduction rate of a single pass is controlled at more than 20% for at least two passes. When the thickness of the rolled piece is 105mm (3.5 times the thickness of the finished product), the second-stage finishing rolling is carried out, the starting rolling temperature is 1080°C, the final rolling temperature is 879°C, and the thickness of the finished steel plate is 30mm. After rolling, the steel plate enters the accelerated cooling equipment, the surface reddening temperature is 169°C, and the offline stacking is more than 72 hours to obtain a 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance.
[0037] Conventional mechanical properties, series impact tests, surface and core hardness tests, and bending properties tests were performed on the steel plates of inventive examples 1 to 3. The results are shown in Table 2.
[0038] Table 2 Mechanical properties of the steel plates of Examples 1 to 3 of the present invention
[0039]
[0040] It can be seen from Table 1 and Table 2 that the 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance of the present invention has good wear resistance and corrosion resistance, and the surface and core hardness also meet the requirement of (HBW10 / 3000) 360, the full thickness wear resistance is good, and the cold bending processing performance is also good.
[0041] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance, characterized in that: Its chemical composition is C: 0.11-0.15%, Si: 0.20-0.50%, Mn: 1.00-1.35%, P: 0.02%-0.07%, S≤0.003%Als: 0.017-0.032%, B: 0.0006-0.0016%, rare earth Re: 0.001-0.02%, Nb, V, Ti, Cr, Mo, Cu, Ni alloy elements are selectively added, 0.010%≤Nb+V+Ti≤0.095%, 0.7%≤Cr+Mo+Cu +Ni≤2.0%, and the balance is Fe and unavoidable impurities; The production method includes: 1) Smelting The molten iron and high-quality scrap steel that have been pre-treated by KR desulfurization are used as raw materials. The bottom blowing of the converter adopts the full-process argon blowing mode, and the end point is hit once to reduce the increase of nitrogen in the molten steel due to supplementary blowing; the LF ladle refining furnace further deoxidizes, desulfurizes, removes inclusions, adjusts the composition and temperature, and strictly controls the argon blowing intensity. The argon blowing curve is formulated according to the principle of strong in the early stage, relatively strong in the middle stage, and weak in the late stage. While ensuring deoxidation, deep desulfurization, and alloying, the secondary oxidation and nitrogen increase in the refining process are reduced; the RH process adopts a circulating deep degassing process to significantly reduce the hydrogen, oxygen, and nitrogen gas content while ensuring the stability of the molten steel temperature, reducing the adverse effects of harmful gases on steel quality. The rare earth lanthanum-cerium alloy is added from the vacuum chute 3-5 minutes before the vacuum treatment is completed and re-pressurized to ensure the rare earth recovery rate; 2) Continuous casting The continuous casting machine is a straight arc continuous casting machine, which adopts argon blowing protection for the large and medium ladle water inlets, dynamic soft pressure reduction at the end of solidification, 380A high current electromagnetic stirring and optimized dynamic secondary cooling technology. Through constant temperature and constant casting speed process, taking into account this low superheat casting, the center segregation, center looseness, cracks and vibration marks of the continuous casting billet are reduced. Finally, high-quality slabs with a thickness of 250mm and 300mm are produced according to the thickness of the finished product; 3) Heating The steel slab is heated in a heating furnace to fully ensure the heating temperature and soaking time of the steel slab; the heating temperature is controlled at 1200℃~1250℃, the heating time is controlled at 220-300min, and the holding time is greater than 60min to ensure sufficient solid solution of alloy elements and uniform temperature of the slab; 4) High temperature rolling The rolling adopts austenite zone rolling, and the deformation of each pass is increased during rough rolling. The thickness is greater than 30mm and the rolling method of transverse rolling + longitudinal rolling is adopted. The slab length is widened to ensure the reduction rate of the extension pass and improve the uniformity of the transverse and longitudinal microstructures. The starting rolling temperature is 1190-1250℃, and the relative reduction rate of a single pass is controlled at least 20% for more than two passes; the deformation of each pass is strictly controlled in the finishing rolling stage, the finishing rolling starting temperature is ≥1050℃, and the starting rolling thickness is set to 2.0-3.5 times the finished product thickness according to the finished product thickness requirements. The rolling speed is 2.0m / s-5.0m / s, and the austenite temperature is calculated according to the composition. The final rolling temperature is 860-930℃, which is 20℃ above the austenite temperature. 5) Rapid cooling The steel plate is rapidly cooled after rolling. According to the martensitic transformation temperature and plate shape control, the roller speed, water pressure and water volume are controlled to achieve a surface red-return temperature of 150℃~350℃ after cooling.
2. The 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance according to claim 1, characterized in that: Its chemical composition by weight percentage is C: 0.15%, Si: 0.20%, Mn: 1.0%, P: 0.020%, S: 0.001%, Als: 0.030%, B: 0.0016%, rare earth Re: 0.001%, Nb: 0.01%, Ti: 0.055%, Cr: 0.4%, Cu: 0.31%, Ni: 0.25%, and the balance is Fe and unavoidable impurities.
3. The 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance according to claim 1, characterized in that: Its chemical composition by weight percentage is C: 0.14%, Si: 0.25%, Mn: 1.10%, P: 0.025%, S: 0.002%, Als: 0.025%, B: 0.0012%, rare earth Re: 0.012%, Nb: 0.01%, Ti: 0.012%, Cr: 0.5%, Cu: 0.28%, Ni: 0.28%, and the balance is Fe and unavoidable impurities.
4. The 1100MPa grade rare earth wide and thick steel plate with both wear resistance and corrosion resistance according to claim 1, characterized in that: Its chemical composition by weight percentage is C: 0.11%, Si: 0.40%, Mn: 1.18%, P: 0.060%, S: 0.003%, Als: 0.017%, B: 0.0006%, rare earth Re: 0.015%, Ti: 0.015%, Cr: 0.48%, Cu: 0.25%, Ni: 0.30%, and the balance is Fe and inevitable impurities.
Citation Information
Patent Citations
Abrasion resistant steel plate having low-temperature toughness, and manufacturing method therefor
CN107354382A
Wear-resisting steel plate with good -60 DEG C ultralow-temperature impact toughness and production method of wear-resisting steel plate
CN110184532A
High-wear-resistance martensite / austenite biphasic wear-resistant steel plate and manufacturing method thereof
CN110592491A
Corrosion resistant wear resistant steel plate and preparation method thereof
CN104611639A
Abrasion resistant steel plate having low-temperature toughness, and manufacturing method therefor