Preparation method of single atomic layer two-dimensional nitride

Through physical vapor deposition method and plasma replacement technology, the problem of difficulty in growing single atomic layer two-dimensional nitride in the existing technology has been solved, efficient nitride semiconductor preparation has been achieved, material damage has been reduced, and material application fields have been broadened.

CN116288276BActive Publication Date: 2024-10-18SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310285066.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-18
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

It is difficult to grow two-dimensional nitride semiconductors at the single atomic layer level with existing technology, and traditional chemical vapor deposition methods result in poor nitridation effects and serious material damage.

Method used

The physical vapor deposition method is used to prepare a precursor template of a single atomic layer on the substrate by controlling the gas delivery flow rate, temperature rise curve and reaction time during the reaction process, and N plasma is used to replace non-group III-V atoms to form single atoms. Layer two-dimensional nitride and use H plasma etching to reduce template damage.

Benefits of technology

Successfully grown two-dimensional nitride semiconductors at the single atomic layer level, avoiding the problem of bonding with the substrate, reducing template damage, and achieving more accurate material characterization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116288276B_ABST
    Figure CN116288276B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a single atomic layer two-dimensional nitride. When the template method is used to grow the two-dimensional nitride, the method avoids growing a precursor template with a large number of layers, and obtains a perfect single atomic layer thickness by controlling factors such as the gas flow rate, the reaction temperature rise curve, and the distance between the source end and the substrate in the PVT method. In addition, it is possible to avoid serious etching during the entire nitridation process, and it is difficult to obtain a flat single atomic layer nitride with low defects due to severe damage to the template.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of III-V group wide bandgap two-dimensional semiconductors, and in particular to a method for preparing a single atomic layer two-dimensional nitride. Background Art

[0002] Nitride semiconductors are an important family in the third-generation semiconductor family. They have many excellent properties. They have a wide bandgap and are more suitable for making high-temperature, high-frequency, radiation-resistant and high-power electronic devices. They shine in the fields of 5G base stations, new energy vehicles, photovoltaics, etc. At the same time, as the research on two-dimensional materials gradually deepens, the performance they show is becoming more and more abundant, showing many properties that the original bulk materials do not have, further broadening the application field of the materials. Therefore, many people began to combine two-dimensional and nitride semiconductors to study two-dimensional nitride semiconductors.

[0003] Two-dimensional nitride semiconductors have many excellent properties, including wider bandgap, excellent mechanical strain capacity, better optical transmittance, ultra-low thermal conductivity, etc. There have been many studies on theoretical calculations of two-dimensional nitride semiconductors, and there have also been some studies on growing thin-layer nitrides. However, the grown two-dimensional nitrides are either in the interlayer, making it difficult to characterize their properties in depth, or they are bonded to the substrate, making it impossible to fully and accurately characterize their properties. There has been no substantial progress in the research on growing ideal self-supporting and single-atomic-layer two-dimensional nitrides. If a self-supporting single-atomic-layer two-dimensional nitride can be grown, it can be peeled off and the properties of the single-atomic-layer nitride semiconductor can be studied in depth without being affected by other surrounding materials.

[0004] In order to obtain a single atomic layer of nitride semiconductors, many researchers have tried to use the template method to obtain two-dimensional nitrides by replacing atoms. This method can obtain reaction precursors that are not bonded to the substrate, and then obtain nitrides that are not bonded to the substrate. However, their templates are far from reaching the single atomic layer level, and the nitride nitridation effect of the traditional chemical vapor deposition (CVD) method is poor and the damage is also great. Therefore, a better template nitridation method is urgently needed.

[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a single atomic layer two-dimensional nitride, which can overcome the technical problem in the prior art that a single atomic layer level template cannot be obtained.

[0007] To achieve the above object, an embodiment of the present invention provides a method for preparing a single atomic layer of two-dimensional nitride, comprising:

[0008] A reaction device is provided, the reaction device comprising a first reaction chamber and a second reaction chamber connected to each other;

[0009] Placing a III-VI group compound evaporation source in a first reaction chamber and placing a growth substrate in a second reaction chamber;

[0010] The evaporation source is heated to transport the evaporated III-VI group atomic gas to the surface of the growth substrate to form a single atomic layer template on the surface of the growth substrate. The gas flow rate range during the gas transport process is 10sccm-50sccm, and the growth time of the III-VI group atoms on the surface of the growth substrate is 5min-10min.

[0011] The single atomic layer template is transferred to a plasma generating device, and non-III-V group atoms in the single atomic layer template are replaced by N atoms to form a single atomic layer of two-dimensional nitride.

[0012] In one or more embodiments, the evaporation source is Ga metal and Ga2Se3, and the molar ratio of Ga metal to Ga2Se3 is in the range of 1:10 to 1:100.

[0013] In one or more embodiments, the evaporation source is heated to meet the following conditions: first, the temperature is increased to 350-450°C at 5-20°C / min, maintained for 5-10 min, then the temperature is increased to 650-750°C at 5-10°C / min, maintained for 5-10 min, then the temperature is increased to 800-920°C at 1-7°C / min and maintained for 5-10 min.

[0014] In one or more embodiments, the evaporation source is GaS powder, and the evaporation source is heated to meet the following conditions: heating to 800-900° C. at a heating rate of 0.1-1° C. / min and then heating for 5 min-10 min.

[0015] In one or more embodiments, the distance between the evaporation source and the growth substrate is controlled within a range of 5 cm to 15 cm.

[0016] In one or more embodiments, a valve is disposed between the first reaction chamber and the second reaction chamber, and the valve is capable of adjusting the flow rate of gas passing through the first reaction chamber.

[0017] In one or more embodiments, in the plasma generating device, H plasma and N plasma are introduced simultaneously, and the flow rate of the N plasma is greater than the flow rate of the H plasma.

[0018] In one or more embodiments, the flow rate of the N plasma is 1 sccm-10 sccm, the flow rate of the H plasma is 0.1 sccm-1 sccm, and the ratio of N atoms to H atoms is controlled at 10:1-20:1.

[0019] In one or more embodiments, the single atomic layer template is a single atomic layer of GaS, InS, GaSe, InSe, GaTe or InTe.

[0020] In one or more embodiments, the gas used in the gas transportation process is nitrogen or argon.

[0021] Compared with the prior art, the present invention adopts a physical vapor deposition (PCT) method, and can prepare a single atomic layer precursor template on a substrate by controlling conditions such as gas delivery flow, reaction temperature rise curve and reaction time during the reaction process. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a schematic structural diagram of a reaction device according to one embodiment of the present invention;

[0023] Figure 2 1 is a schematic diagram of the structure of a valve in a reaction device according to an embodiment of the present invention, wherein (1) to (4) are schematic diagrams of the valve apertures becoming smaller in sequence;

[0024] Figure 3 1 is a schematic diagram of the principle of replacing non-III-V group atoms in a single atomic layer template with N atoms according to an embodiment of the present invention;

[0025] Figure 4 Schematic diagram of the GaSe template obtained in Example 1 of the present invention, wherein (a) is a single-layer GaSe template obtained by AFM scanning, and (b) is the thickness of the single atomic layer of GaSe corresponding to the template;

[0026] Figure 5 are SEM images and CL images of the template obtained in Comparative Example 4, wherein (a) refers to the SEM morphology image of the thicker GaSe grown without using the specified parameters, and (b) is the corresponding CL image;

[0027] Figure 6 3 are morphology images of the template after being etched by H atoms, wherein a) is the morphology image of the template after being etched in Example 1, and b) is the morphology image of the template after being etched in Comparative Example 7. DETAILED DESCRIPTION

[0028] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.

[0029] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.

[0030] like Figure 1 As shown, a reaction device 10 according to a preferred embodiment of the present invention includes a first reaction chamber 11 and a second reaction chamber 12 that are connected to each other, and a valve 13 disposed between the first reaction chamber 11 and the second reaction chamber 12 .

[0031] The reaction device 10 is used to realize physical vapor deposition (PVT), wherein the first reaction chamber 11 is used as a source end to place an evaporation source 20, and the second reaction chamber 12 is used as a growth end to place a growth substrate 30. When the steam flow in the first reaction chamber 11 is transported to the second reaction chamber 12 by gas transport, the valve 13 is used to control the flow rate of the gas transport, thereby adjusting the steam flow rate flowing through the growth substrate 30.

[0032] Ginseng Figure 2 As shown, in a preferred embodiment, the aperture of the valve 13 is adjustable, and a plurality of shielding plates are used, which is similar to the structure of a camera aperture, and the amount of gas flowing through can be controlled by changing the aperture size.

[0033] The embodiment of the present invention also discloses a method for preparing a single atomic layer two-dimensional nitride, comprising:

[0034] Step s1, providing Figure 1 The reaction device 10 is shown.

[0035] Step s2 , placing a III-VI compound evaporation source 20 in the first reaction chamber 11 , and placing a growth substrate 30 in the second reaction chamber 12 .

[0036] The distance between the evaporation source 20 and the growth substrate 30 is 5 cm-15 cm.

[0037] When GaSe is used as the evaporation source 20 , the raw materials are Ga metal and Ga2Se3, and the ratio is in the range of 1:10 to 1:100, or the ratio of GaSe to Ga2Se3 is between 100:1 and 10:1.

[0038] Step s3, heating the evaporation source.

[0039] When GaSe is used as the evaporation source 20, the heating conditions are as follows: first, the temperature is raised to 350-450°C at 5-20°C / min, maintained for 5-10min, then the temperature is raised to 650-750°C at 5-10°C / min, maintained for 5-10min, then the temperature is raised to 800-920°C at 1-7°C / min, maintained for 5min-10min.

[0040] When GaS powder is selected as the evaporation source, the heating conditions are as follows: heating to 800-900°C at a heating rate of 0.1-1°C / min and then heating for 5min-10min.

[0041] In step s4, the evaporated II-VI group atoms are transported to the surface of the growth substrate 30 through gas to form a single atomic layer template on the surface of the growth substrate 30. The gas flow rate range of the gas transport process is controlled by a valve to be 10sccm-50sccm. The transport gas can be nitrogen or argon. The growth time of III-VI group atoms on the surface of the growth substrate is 5min-10min.

[0042] Step s5, transferring the single atomic layer template to a plasma generating device, Figure 3 As shown, N atoms replace non-III-V group atoms in the single atomic layer template to form a single atomic layer of two-dimensional nitride. Figure 3 (a) is a schematic diagram before atomic replacement. The circle in the figure is the atomic vacancies left after non-III-V group atoms are etched by H-plasma. Figure 3 (b) is a schematic diagram after atomic replacement, where the position in the circle is the atomic replacement diagram after the vacancy is immediately filled with N atoms.

[0043] Step s6, after nitridation is completed, keep warm for 10 minutes to 60 minutes to allow the atoms to fully relax.

[0044] In the above step s2, the growth substrate 30 may be a Si substrate, a sapphire substrate or a metal substrate.

[0045] In the above step s4, the single atomic layer template includes a series of III-VI group compounds such as GaS, InS, GaSe, InSe, GaTe, and InTe.

[0046] In the above step s5, H plasma and N plasma are introduced into the plasma generator at the same time, and the flow rate of the N plasma is greater than the flow rate of the H plasma. The flow rate of the N plasma is 1 sccm-10 sccm, the flow rate of the H plasma is 0.1 sccm-1 sccm, and the ratio of N atoms to H atoms is controlled to be 10:1-20:1.

[0047] In some embodiments, H plasma may be introduced for a certain period of time before N plasma is introduced.

[0048] In the above step s5, the plasma generating device needs to be fed with N plasma in an ultra-vacuum environment, where the ultra-vacuum refers to a vacuum degree better than 1*10 -5 torr.

[0049] In this technical solution, in order to solve the serious problem of nitridation etching, this embodiment provides a method of nitridation with N-plasma and a small amount of H-plasma assisted nitridation. The etching of a small amount of H-plasma promotes the non-III-V group atoms to leave the template surface, and the excess N-plasma will immediately fill in the vacancies to complete the replacement. Since there are few H atom sources, the etching effect caused by it is very weak, and the vacancies are immediately replaced by N atoms, which is not easy to have too much etching effect on the surface.

[0050] Example 1

[0051] The single atomic layer template uses GaSe.

[0052] The single crystal Si substrate 30 is cleaned and placed in the second reaction chamber 12 of the reaction device 10 .

[0053] Place the III-VI group compound evaporation source 20 in the first reaction chamber 11 of the reaction device 10, and the distance between the evaporation source 20 and the growth substrate 30 is 10 cm. The specific evaporation source 20 can be Ga droplets and Ga2Se3, with a molar ratio of 1:10. Adjust the aperture of the intermediate valve 13 to an appropriate size, control the gas flow rate to 10sccm during gas delivery, set the heating curve, and start heating. Heating curve control method: first increase the temperature to 400℃ at 20℃ / min, maintain for 10min, then increase the temperature to 700℃ at 10℃ / min, maintain for 10min, then increase the temperature to 920℃ at 7℃ / min, then stop heating and maintain stable growth for 5min. The final GaSe template thickness is 0.8nm, which is exactly the thickness of a single layer, such as Figure 4 As shown, (a) is a single-layer GaSe template obtained by AFM scanning, and the right figure (b) is the single atomic layer thickness of GaSe corresponding to the template.

[0054] The obtained single atomic layer template is transferred to the N-plasma equipment through a vacuum pipeline. When the temperature rises to the set temperature of about 920℃, a certain amount of N-plasma is introduced and a small amount of H-plasma is used to promote the incorporation of N atoms to prepare a III-V group single atomic layer compound. The flow rate of N plasma is 10sccm, and the flow rate of H plasma is 1sccm. The image parameters after template etching are Figure 6 (a)

[0055] After nitridation is completed, keep the temperature at around 920℃ for 10 minutes to allow the atoms to fully relax.

[0056] Example 2

[0057] The single atomic layer template uses GaSe.

[0058] The single crystal Si substrate 30 is cleaned and placed in the second reaction chamber 12 of the reaction device 10 .

[0059] Place the III-VI group compound evaporation source 20 in the first reaction chamber 11 of the reaction device 10, and the distance between the evaporation source 20 and the substrate is 10 cm. The specific evaporation source 20 can be GaSe and Ga2Se3, with a molar ratio of 10:1. Adjust the aperture of the intermediate valve 13 to a suitable size, control the gas flow rate during the gas delivery process to 10 sccm, set the heating curve, and start heating. Heating curve control method: first heat to 400℃ at 20℃ / min, maintain for 10min, then heat to 700℃ at 10℃ / min, maintain for 10min, then heat to 900℃ at 7℃ / min, then stop heating and maintain stable growth for 10min. The final GaSe template thickness is 0.8nm, which is exactly the thickness of a single layer.

[0060] The obtained single atomic layer template is transferred to the N-plasma equipment through a vacuum pipeline. When the temperature rises to the set temperature of about 900°C, a certain amount of N-plasma is introduced and a small amount of H-plasma is used to promote the incorporation of N atoms to prepare a III-V group single atomic layer compound, wherein the flow rate of N plasma is 10sccm and the flow rate of H plasma is 1sccm.

[0061] After nitridation is completed, keep the temperature at about 900℃ for 10 minutes to allow the atoms to fully relax.

[0062] Example 3

[0063] The single atomic layer template uses GaS.

[0064] The single crystal Si substrate 30 is cleaned and placed in the second reaction chamber 12 of the reaction device 10 .

[0065] Place the III-VI group compound evaporation source 20 in the first reaction chamber 11 of the reaction device 10. The specific evaporation source 20 can be GaS powder. Adjust the aperture of the intermediate valve 13 to a suitable size, control the gas flow rate to 30 sccm during the gas delivery process, set the heating curve, and start heating. The heating curve control method is: heat up at a heating rate of 1°C / min, and after heating to 900°C, keep heating at this temperature for 10 minutes. Finally, a single-layer GaS template is obtained.

[0066] The obtained single atomic layer template is transferred to the N-plasma equipment through a vacuum pipeline. When the temperature rises to 800°C, a certain amount of N-plasma is introduced and a small amount of H-plasma is used to promote the incorporation of N atoms to prepare a III-V group single atomic layer compound, wherein the flow rate of N plasma is 3sccm and the flow rate of H plasma is 0.2sccm.

[0067] After nitridation is completed, the optimal temperature is maintained at 800℃ for 60 minutes to allow the atoms to fully relax.

[0068] Example 4

[0069] The single atomic layer template uses InSe.

[0070] The single crystal Si substrate 30 is cleaned and placed in the second reaction chamber 12 of the reaction device 10 .

[0071] Place the III-VI compound evaporation source 20 in the first reaction chamber 11 of the reaction device 10, and the distance between the evaporation source 20 and the growth substrate 30 is 15 cm. The specific evaporation source 20 can be In particles and Se powder, and the molar ratio of the two is 1:1. Adjust the aperture of the intermediate valve 13 to a suitable size, control the gas flow rate during gas delivery to 50sccm, set the heating curve, and start heating. Heating curve control method: heat up to 900℃ at a heating rate of 5℃ / min, grow stably within the terminal temperature range for 8min, and finally obtain a single-layer InSe template.

[0072] The obtained single atomic layer template is transferred to the N-plasma equipment through a vacuum pipeline. When the temperature rises to the set temperature of 800°C, a certain amount of N-plasma is introduced and a small amount of H-plasma is used to promote the incorporation of N atoms to prepare a III-V group single atomic layer compound, wherein the flow rate of N plasma is 10 sccm and the flow rate of H plasma is 1 sccm.

[0073] After nitridation, keep the temperature at 800℃ for 20 minutes to allow the atoms to fully relax.

[0074] Example 5

[0075] InS was used as the single atomic layer template.

[0076] The sapphire substrate 30 is cleaned and placed in the second reaction chamber 12 of the reaction device 10 .

[0077] Place the III-VI compound evaporation source 20 in the first reaction chamber 11 of the reaction device 10, and the distance between the evaporation source 20 and the growth substrate 30 is 5 cm. The specific evaporation source 20 can be S powder and In2O3, and the molar ratio of the two is 2:1. Adjust the aperture of the intermediate valve 13 to a suitable size, control the gas flow rate during the gas delivery process to 10sccm, set the heating curve, and start heating. Heating curve control method: heat up to 700℃ at a heating rate of 5℃ / min, and grow stably within the terminal temperature range for 10min. Finally, a single-layer InS template is obtained.

[0078] The obtained single atomic layer template is transferred to the N-plasma equipment through a vacuum pipeline. When the temperature rises to the set temperature of 600°C, a certain amount of N-plasma is introduced and a small amount of H-plasma is used to promote the incorporation of N atoms to prepare a III-V group single atomic layer compound, wherein the flow rate of N plasma is 1 sccm and the flow rate of H plasma is 0.1 sccm.

[0079] After nitridation is completed, keep the temperature at around 600℃ for 20 minutes to allow the atoms to fully relax.

[0080] Example 6

[0081] The single atomic layer template is GaTe.

[0082] The single crystal Si substrate 30 is cleaned and placed in the second reaction chamber 12 of the reaction device 10 .

[0083] Place the III-VI compound evaporation source 20 in the first reaction chamber 11 of the reaction device 10, and the distance between the evaporation source 20 and the growth substrate 30 is 10 cm. The specific evaporation source 20 can be Ga droplets and Te, and the molar ratio of the two is 1:1. Adjust the aperture of the intermediate valve 13 to a suitable size, control the gas flow rate during gas delivery to 10sccm, set the heating curve, and start heating. Heating curve control method: first increase the temperature from room temperature to 500℃ at 50℃ / h, then increase the temperature to 750℃ at 10℃ / min, and finally increase the temperature to 950℃ at 5℃ / min, and grow stably for 7min within the terminal temperature range. Finally, a single-layer GaTe template is obtained.

[0084] The obtained single atomic layer template is transferred to the N-plasma equipment through a vacuum pipeline. When the temperature rises to the set temperature of 800°C, a certain amount of N-plasma is introduced and a small amount of H-plasma is used to promote the incorporation of N atoms to prepare a III-V group single atomic layer compound, wherein the flow rate of N plasma is 8sccm and the flow rate of H plasma is 0.5sccm.

[0085] After nitridation is completed, keep the temperature at around 800℃ for 20 minutes to allow the atoms to fully relax.

[0086] Example 7

[0087] The single atomic layer template uses InTe.

[0088] The single crystal Si substrate 30 is cleaned and placed in the second reaction chamber 12 of the reaction device 10 .

[0089] Place the III-VI compound evaporation source 20 in the first reaction chamber 11 of the reaction device 10, and the distance between the evaporation source 20 and the growth substrate 30 is 10 cm. The specific evaporation source 20 can be In particles and Te single substance, and the molar ratio of the two is 1:1. Adjust the aperture of the intermediate valve 13 to a suitable size, control the gas flow rate during gas delivery to 10sccm, set the heating curve, and start heating. Heating curve control method: heat up to 700℃ at a heating rate of 5℃ / min, and grow stably within the terminal temperature range for 5min. Finally, a single-layer InTe template is obtained.

[0090] The obtained single atomic layer template is transferred to the N-plasma equipment through a vacuum pipeline. When the temperature rises to the set temperature of 700°C, a certain amount of N-plasma is introduced and a small amount of H-plasma is used to promote the incorporation of N atoms to prepare a III-V group single atomic layer compound, wherein the flow rate of N plasma is 10 sccm and the flow rate of H plasma is 1 sccm.

[0091] After nitridation is completed, keep the temperature at around 700℃ for 20 minutes to allow the atoms to fully relax.

[0092] Comparative Example

[0093] The parameters such as the heating curve, stable growth time, gas flow rate, N plasma flow rate, H plasma flow rate, etc. were changed. Other experimental conditions were the same as those in Example 1. The effects are compared in Table 1.

[0094] Table 1

[0095]

[0096]

[0097] It can be seen from Comparative Examples 1 and 2 that the parameters of the heating curve have an impact on the formation of the single-layer template, wherein if the growth temperature is too low, the single crystal state cannot be maintained, and an amorphous state and a polycrystalline state will appear.

[0098] From Comparative Examples 3 and 4, it can be seen that the material growth time (the time maintained after heating to the highest temperature) affects the formation of the single-layer template. When the growth time is too short, a uniform film cannot be formed. When the growth time is too long, the obtained template is very thick. Figure 5 shown.

[0099] It can be seen from Comparative Examples 5 and 6 that the flow rate of gas delivery during the growth process has an impact on the formation of a single-layer template. Among them, a too low carrier gas volume will cause the mass transfer process to be unable to proceed or progress too slowly. A too high carrier gas volume will cause the template to grow in a layer-first, island-later growth pattern, and its layered growth cannot be controlled.

[0100] It can be seen from Comparative Examples 7 and 8 that when the content of H plasma is too high, the etching phenomenon is serious during the entire nitridation process, the template is seriously damaged, and the Figure 6 (b)

[0101] In summary, when the present invention uses the template method to grow two-dimensional nitride, it avoids growing a precursor template with a large number of layers, but continuously adjusts the thickness of the growing precursor template by controlling the gas flow rate, reaction temperature rise curve, the distance between the source end and the substrate in the PVT method, etc., until a perfect single atomic layer thickness is reached. In addition, it is possible to avoid serious etching during the entire nitridation process, and it is difficult to obtain a flat, low-defect single atomic layer nitride due to severe damage to the template.

[0102] The foregoing description of specific exemplary embodiments of the present invention is

[0103] For the purpose of illustration and description. These descriptions are not intended to limit the invention to the precise form disclosed, and it is obvious that many changes and variations can be made in light of the above teachings. The exemplary embodiments are selected and described for the purpose of explaining the specific principles of the invention and its practical application, so that those skilled in the art can make and utilize various different exemplary embodiments of the invention and various different options and changes. The scope of the invention is intended to be defined by the claims and their equivalents.

Claims

1. A method for preparing a single atomic layer of two-dimensional nitride, It is characterized in that include: A reaction device is provided, comprising a first reaction chamber and a second reaction chamber connected to each other; Placing a III-VI group compound evaporation source in a first reaction chamber and placing a growth substrate in a second reaction chamber; The evaporation source is heated to transport the evaporated III-VI group atomic gas to the surface of the growth substrate to form a single atomic layer template on the surface of the growth substrate. The gas flow rate range of the gas transport process is 10sccm-50sccm, the growth time of the III-VI group atoms on the surface of the growth substrate is 5min-10min, and the distance between the evaporation source and the growth substrate is controlled in the range of 5cm-15cm; The single atomic layer template is transferred to a plasma generator, and non-Group III-V atoms in the single atomic layer template are replaced by N atoms to form a single atomic layer two-dimensional nitride. In the plasma generator, H plasma and N plasma are introduced simultaneously, and the flow rate of the N plasma is greater than the flow rate of the H plasma. The flow rate of the N plasma is 1 sccm-10 sccm, and the flow rate of the H plasma is 0.1 sccm-1 sccm. The ratio of N atoms to H atoms is controlled to be 10:1-20:

1. When the evaporation source is Ga metal and Ga 2 Se 3 When Ga metal and Ga 2 Se 3 The molar ratio is within the range of 1:10 to 1:100, and the heating conditions of the evaporation source are as follows: firstly, the temperature is increased to 350-450°C at 5-20°C / min, maintained for 5-10min, then the temperature is increased to 650-750°C at 5-10°C / min, maintained for 5-10min, then the temperature is increased to 800-920°C at 1-7°C / min, and maintained for 5-10min; When the evaporation source is GaS powder, the evaporation source is heated to meet the following conditions: heating to 800-900° C. at a heating rate of 0.1-1° C. / min and then heating for 5 min-10 min.

2. The method for preparing a single atomic layer two-dimensional nitride according to claim 1, It is characterized in that A valve is provided between the first reaction chamber and the second reaction chamber, and the flow rate of the gas passing through the valve is adjustable.

3. The method for preparing a single atomic layer two-dimensional nitride according to claim 1, It is characterized in that The single atomic layer template is a single atomic layer of GaS, InS, GaSe, InSe, GaTe or InTe.

4. The method for preparing a single atomic layer two-dimensional nitride according to claim 1, It is characterized in that The gas used in the gas transportation process is nitrogen or argon.

Citation Information

Patent Citations

  • Surface nitrogen passivation method of semiconductor material

    CN108364851A

  • Method for preparing GaN film on two-dimensional graphite substrate

    CN108511322A