A method for improving the nitric acid dissolution performance of uranium peroxide products
By stirring uranium octoxide and uranium peroxide products in a nitric acid solution, the nitric acid dissolution performance is improved, the problem of high temperature and long time dissolution of uranium peroxide products is solved, efficient uranium product dissolution is achieved, and the process economy is improved.
Patent Information
- Application Number
- CN202111618477.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-12-27
AI Technical Summary
The process of dissolving uranium peroxide products in nitric acid is high and takes a long time, which affects the economic benefits of the process.
Stir and dissolve the uranium octoxide product and uranium peroxide product in the nitric acid solution. The molar ratio is not less than 1. The concentration of the nitric acid solution is not less than 2.5 mol/L. Heat to 50°C and the stirring time is not less than 15 minutes. Raise the nitric acid solution. uranium content.
The dissolution temperature of nitric acid is reduced, the dissolution rate is increased, a uranium product dissolution rate of 98.8% is achieved, and the dissolution time is shortened to 15 minutes.
Abstract
Description
Technical Field
[0001] The invention relates to the field of uranium purification and conversion, and in particular to a method for improving the nitric acid dissolution performance of uranium peroxide products. Background Art
[0002] The nitric acid dissolution of uranium concentrate is the first step in the uranium purification and conversion process, and its importance can be seen. At present, nitric acid is basically used to dissolve uranium ore concentrate internationally.
[0003] Uranium peroxide (UO4) is a common uranium concentrate product. It is a uranium oxide product directly prepared by H2O2 precipitation. Compared with the conventional U3O8 product form, the preparation process of UO4 product is simple, no calcination is required, and the reagents are more environmentally friendly, but its nitric acid solubility is much lower than that of U3O8 products. Uranium peroxide product is UO2 2+ With O2 2- Uranium compounds obtained by complexation, O2 2- It is highly oxidizing and cannot be dissolved by nitric acid through chemical reactions. It can only be dissolved by high temperature. 2- Decomposition achieves the purpose of dissolution. To prepare a uranium solution with a concentration of 300g / L, the dissolution temperature needs to be raised to 80°C and the dissolution time is 1 hour. Under the same conditions, the nitric acid dissolution temperature of U3O8 is 50°C and the time is 15 minutes. The nitric acid dissolution performance of uranium peroxide has become one of the main factors restricting the promotion of its process. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for improving the nitric acid dissolution performance of uranium peroxide products, thereby reducing the dissolution temperature, shortening the dissolution time and improving the process economic benefits.
[0005] The present invention provides a method for improving the nitric acid solubility of a uranium peroxide product, comprising the following steps:
[0006] Adding the uranium trioxide product and the uranium peroxide product into the nitric acid solution and stirring to dissolve;
[0007] The molar ratio of the uranium octoxide product to the uranium peroxide product is not less than 1;
[0008] The concentration of the nitric acid solution is not less than 2.5 mol / L.
[0009] Preferably, it specifically includes:
[0010] Heat the nitric acid solution;
[0011] The uranium trioxide product and the uranium peroxide product are premixed and added to the heated nitric acid solution.
[0012] Preferably, the heating temperature does not exceed 50°C.
[0013] Preferably, the stirring and dissolving time is not less than 15 minutes.
[0014] Preferably, the concentration of the nitric acid solution is 3-6 mol / L.
[0015] Preferably, the uranium content of the uranium trioxide product is not less than 84.8%.
[0016] Preferably, the uranium content of the uranium peroxide product is not less than 70.1%.
[0017] Compared with the prior art, the method of improving the nitric acid solubility of uranium peroxide products of the present invention reduces the dissolution temperature of UO4 in the nitric acid dissolution process and increases the dissolution rate of UO4 in the nitric acid dissolution process by dissolving uranium trioxide products and uranium peroxide products in combination. The technology is economical, simple and practical. DETAILED DESCRIPTION
[0018] In order to further understand the present invention, the embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the present invention.
[0019] The embodiment of the present invention discloses a method for improving the nitric acid solubility of a uranium peroxide product, comprising the following steps:
[0020] Adding the uranium trioxide product and the uranium peroxide product into the nitric acid solution and stirring to dissolve;
[0021] The molar ratio of the uranium octoxide product to the uranium peroxide product is not less than 1;
[0022] The concentration of the nitric acid solution is not less than 2.5 mol / L, preferably 3 to 6 mol / L.
[0023] Preferably, it specifically includes:
[0024] Heat the nitric acid solution;
[0025] The uranium trioxide product and the uranium peroxide product are premixed and added to the heated nitric acid solution.
[0026] The heating temperature does not exceed 50°C.
[0027] The stirring and dissolving time is not less than 15 minutes.
[0028] The uranium content of the uranium trioxide product is not less than 84.8%.
[0029] The uranium content of the uranium peroxide product is not less than 70.1%.
[0030] The present invention 1) reduces the dissolution temperature of UO4 during the dissolution process of nitric acid.
[0031] O2 in UO4 material 2- As a strong oxidant, nitric acid cannot completely dissolve UO4 through acid hydrolysis, so it is necessary to increase the temperature to make O2 2- Decompose to achieve the purpose of dissolving UO4. The invention dissolves the UO4 material by mixing it with the U3O8 material. 2- It undergoes redox reaction with +4 uranium in U3O8 material to convert O2 2- Reduction to O 2- The dissolution process only needs to maintain a normal temperature of 50°C to quickly dissolve UO4. The invention effectively reduces the dissolution temperature of UO4 during the nitric acid dissolution process.
[0032] 2) The dissolution rate of UO4 in the nitric acid dissolution process was improved.
[0033] The invention dissolves the O2 in the UO4 material by mixing it with the U3O8 material. 2- The redox reaction takes place with the +4 uranium in the U3O8 material, and the rate of the redox reaction is much higher than the rate of the thermal decomposition reaction. Therefore, the invention can effectively increase the dissolution rate of UO4 during the nitric acid dissolution process.
[0034] In order to further understand the present invention, the method for improving the nitric acid solubility of uranium peroxide products provided by the present invention is described in detail below in conjunction with examples, and the protection scope of the present invention is not limited by the following examples.
[0035] Example 1
[0036] 100ml of nitric acid solution with a concentration of 6moL / L is used, the uranium content is calculated at a concentration of 300g / L, the molar ratio of U3O8 to UO4 products is 1:1, the uranium content of U3O8 products is 84.8%, and the uranium content of UO4 products is 70.1%, that is, 26.5g of U3O8 products and 10.7g of UO4 products need to be added to 100mol of nitric acid solution. The nitric acid solution is heated to 50°C using a water bath thermostatic agitator. Subsequently, the pre-mixed U3O8 and UO4 products are added to the nitric acid solution, and the stirring and dissolution time is monitored. After dissolution, the solution is filtered and the insoluble slag is dried and weighed. The dissolution rate of the uranium product is calculated to be 98.85%, and the dissolution time is 15 minutes.
[0037] Example 2
[0038] 100ml of a solution with a nitric acid concentration of 6moL / L is used, and the uranium content is calculated at a concentration of 300g / L. The molar ratio of U3O8 to UO4 products is 1:1, the uranium content of the U3O8 product is 84.8%, and the uranium content of the UO4 product is 70.1%, that is, 26.5g of U3O8 product and 10.7g of UO4 product need to be added to 100mol of nitric acid solution. The nitric acid solution is heated to 50°C using a water bath thermostatic agitator. Subsequently, the U3O8 product is added first, and then the UO4 product is added to the nitric acid solution, and the stirring and dissolution time is monitored. After dissolution, the solution is filtered and the insoluble slag is dried and weighed. The dissolution rate of the uranium product is calculated to be 98.79%, and the dissolution time is 15 minutes.
[0039] Example 3
[0040] 100ml of a solution with a nitric acid concentration of 6moL / L is used, and the uranium content is calculated at a concentration of 300g / L. The molar ratio of U3O8 to UO4 products is 1:1, the uranium content of U3O8 products is 84.8%, and the uranium content of UO4 products is 70.1%, that is, 26.5g of U3O8 products and 10.7g of UO4 products need to be added to 100mol of nitric acid solution. The nitric acid solution is heated to 50°C using a water bath thermostatic agitator. Subsequently, the UO4 product is added first, and then the U3O8 product is added to the nitric acid solution, and the stirring and dissolution time is monitored. After dissolution, the solution is filtered and the insoluble slag is dried and weighed. The dissolution rate of the uranium product is calculated to be 98.81%, and the dissolution time is 15 minutes.
[0041] Example 4
[0042] 100ml of a solution with a nitric acid concentration of 3moL / L is used, the uranium content is calculated at a concentration of 300g / L, the molar ratio of U3O8 to UO4 products is 1:1, the uranium content of U3O8 products is 84.8%, and the uranium content of UO4 products is 70.1%, that is, 26.5g of U3O8 products and 10.7g of UO4 products need to be added to 100mol of nitric acid solution. The nitric acid solution is heated to 50°C using a water bath thermostatic agitator. Subsequently, the pre-mixed U3O8 and UO4 products are added to the nitric acid solution, and the stirring and dissolution time is monitored. After dissolution, the solution is filtered and the insoluble slag is dried and weighed. The dissolution rate of the uranium product is calculated to be 98.89%, and the dissolution time is 15 minutes.
[0043] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0044] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for improving the nitric acid solubility of uranium peroxide products, characterized in that: The following steps are involved: Adding the uranium trioxide product and the uranium peroxide product into the nitric acid solution and stirring to dissolve; The molar ratio of the uranium octoxide product to the uranium peroxide product is not less than 1; The concentration of the nitric acid solution is not less than 2.5 mol / L.
2. The method for improving the nitric acid solubility of uranium peroxide products according to claim 1, characterized in that: Specifically include: Heat the nitric acid solution; The uranium trioxide product and the uranium peroxide product are premixed and added to the heated nitric acid solution.
3. The method for improving the nitric acid solubility of uranium peroxide products according to claim 2, characterized in that: The heating temperature does not exceed 50°C.
4. The method for improving the nitric acid solubility of uranium peroxide products according to claim 1, characterized in that: The stirring and dissolving time is not less than 15 minutes.
5. The method for improving the nitric acid solubility of uranium peroxide products according to claim 1, characterized in that: The concentration of the nitric acid solution is 3-6 mol / L.
6. The method for improving the nitric acid solubility of uranium peroxide products according to claim 1, characterized in that: The uranium content of the uranium trioxide product is not less than 84.8%.
7. The method for improving the nitric acid solubility of uranium peroxide products according to claim 1, characterized in that: The uranium content of the uranium peroxide product is not less than 70.1%.
Citation Information
Patent Citations
Yellowcake processing in uranium recovery
US4302428A