A super early strength agent and its preparation method and application
By using a combination of crystal-colloid mixed calcium silicate hydrate, reinforcing agent and modifier in the ultra-early strength agent, the problem of insufficient promotion of dicalcium silicate hydration in the existing technology is solved, and early cement silicate is achieved. And the improvement of late-stage strength significantly improves the effect of super early strength agent.
Patent Information
- Application Number
- CN202310404168.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-17
AI Technical Summary
Existing super early strength agents have a weak hydration-promoting effect on dicalcium silicate, resulting in poor later strength and limited use effect when improving the early strength of cement.
Using a combination of 75 to 80 parts of crystal-colloid mixed calcium silicate hydrate, 4 to 10 parts of reinforcing agent and 15 to 20 parts of modifier, super early strength agent, reinforcing agent and modification are prepared through hydrothermal reaction The agent is intercalated in colloidal calcium silicate hydrate, optimizing the mass ratio of crystalline calcium silicate hydrate and colloidal calcium silicate hydrate, and promoting the simultaneous hydration of tricalcium silicate and dicalcium silicate.
It significantly improves the early and late strength of cement, enhances the use effect of ultra-early strength agent, and is suitable for the manufacture of low-carbon building materials and prefabricated building components. It especially improves the early strength and late stability in concrete construction.
Smart Images

Figure CN116354639B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a super early strength agent and a preparation method and application thereof. Background Art
[0002] Super early strength agents can promote cement hydration and thus improve early strength. They are widely used in construction projects, especially in winter construction or in urgent repair projects. The current super early strength agents are mainly colloidal super early strength agents with a calcium-silicon ratio of 1. The colloidal super early strength agents mainly provide nucleation sites for cement hydration, reduce nucleation potential energy, and promote C3S (tricalcium silicate) hydration to improve the early strength of cement. However, the existing super early strength agents have a weak effect on promoting the hydration of C2S (dicalcium silicate), which greatly reduces the use effect of super early strength agents.
[0003] For example, Chinese patent CN113929341A discloses "a nano-seed super early strength agent suitable for low temperature environment and its preparation method". The super early strength agent disclosed in the patent includes 10-20% calcium source, 5-10% silicon source, 0.5-1.5% high stability suspension dispersant, 5-10% auxiliary early strength agent and 0.05-0.1% pH value regulator; wherein the auxiliary early strength agent is added after the formation of CSH precursor, and finally forms the nano-seed super early strength agent, and the auxiliary early strength agent is used to break the metastable covering layer on the surface of C3S, thereby releasing C3S from agglomeration, thereby playing a synergistic role in accelerating the early hydration of cement, and the early strength is significantly improved and the later strength has no shrinkage, but the early strength agent only promotes the hydration of C3S, and does not consider the promotion effect on C2S. Summary of the invention
[0004] In view of this, the present invention provides an ultra-early strength agent and a preparation method and application thereof. The ultra-early strength agent provided by the present invention can simultaneously promote the hydration of tricalcium silicate and dicalcium silicate, and significantly improve the use effect of the ultra-early strength agent.
[0005] In order to solve the above technical problems, the present invention provides an ultra-early strength agent, comprising the following components in parts by weight:
[0006] 75-80 parts of crystal-colloidal mixed hydrated calcium silicate;
[0007] 4 to 10 parts of enhancer;
[0008] 15-20 parts of modifier;
[0009] The crystalline-colloidal mixed calcium silicate hydrate includes crystalline calcium silicate hydrate and colloidal calcium silicate hydrate; the crystalline calcium silicate hydrate is tobermorite, and the colloidal calcium silicate hydrate is type I CSH gel; the mass ratio of the crystalline calcium silicate hydrate to the colloidal calcium silicate hydrate is 0.35-0.65:1;
[0010] The reinforcing agent and the modifier are intercalated in the colloidal hydrated calcium silicate.
[0011] Preferably, the enhancer is diethanol monoisopropanolamine or calcium formate.
[0012] Preferably, the modifier is potassium sodium tartrate or sodium citrate.
[0013] Preferably, the molar ratio of CaO / SiO2 in the crystalline calcium silicate hydrate is 0.83 to 1:1.
[0014] Preferably, the molar ratio of CaO / SiO2 in the colloidal calcium silicate hydrate is 1.0 to 1.2:1.
[0015] Preferably, the specific surface area of the ultra-early strength agent is 450-500m 2 / kg.
[0016] The present invention also provides a method for preparing the ultra-early strength agent described in the above technical solution, comprising the following steps:
[0017] dissolving the enhancer and the modifier in water to obtain an auxiliary material solution;
[0018] The auxiliary material solution and α-type calcium silicate hydrate are mixed to carry out a hydrothermal reaction to obtain the super early strength agent; the pressure of the hydrothermal reaction is 0.8-1.2 MPa, the temperature of the hydrothermal reaction is 170-190° C., and the time of the hydrothermal reaction is 4-10 hours.
[0019] Preferably, the molar ratio of CaO / SiO2 in the α-type calcium silicate hydrate is 1.5 to 1.9:1.
[0020] The present invention also provides the use of the ultra-early strength agent described in the above technical solution or the ultra-early strength agent prepared by the preparation method described in the above technical solution in a cementitious material.
[0021] Preferably, the mass ratio of the ultra-early strength agent to the gelling material is 0.3-0.6:100.
[0022] The invention provides a super early strength agent, comprising the following components in parts by mass: 75-80 parts of crystal-colloidal mixed calcium silicate hydrate, 4-10 parts of a reinforcing agent and 15-20 parts of a modifier; the crystal-colloidal mixed calcium silicate hydrate comprises crystal calcium silicate hydrate and colloidal calcium silicate hydrate; the crystal calcium silicate hydrate is tobermorite, and the colloidal calcium silicate hydrate is type I CSH gel; the mass ratio of the crystal calcium silicate hydrate to the colloidal calcium silicate hydrate is 0.35-0.65:1; the reinforcing agent and the modifier are intercalated in the colloidal calcium silicate hydrate. The super early strength agent provided by the present invention contains both crystalline calcium silicate hydrate and colloidal calcium silicate hydrate. The mass ratio of crystalline calcium silicate hydrate and colloidal calcium silicate hydrate is limited to the above range, so that the super early strength agent can promote the hydration of tricalcium silicate and dicalcium silicate at the same time, overcome the problem that the colloidal calcium silicate hydrate has a weak promoting effect on the hydration of dicalcium silicate, improve the early strength of the cementitious material while improving the later strength of the cementitious material, and significantly improve the use effect of the super early strength agent. The super early strength agent provided by the present invention is suitable for low-carbon building materials, additive manufacturing of prefabricated building components, and concrete construction with special requirements for early strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the XRD spectrum of the ultra-early strength agent prepared in Example 4;
[0024] Figure 2 This is the SEM image of the super early strength agent prepared in Example 4. DETAILED DESCRIPTION
[0025] The present invention provides an ultra-early strength agent, comprising the following components in parts by weight:
[0026] 75-80 parts of crystal-colloidal mixed hydrated calcium silicate;
[0027] 4 to 10 parts of enhancer;
[0028] 15 to 20 parts of modifier.
[0029] In terms of mass fraction, the ultra-early strength agent provided by the present invention comprises 75 to 80 parts of crystalline-colloidal mixed calcium silicate hydrate, preferably 76 to 78 parts. In the present invention, the crystalline-colloidal mixed calcium silicate hydrate comprises crystalline calcium silicate hydrate and colloidal calcium silicate hydrate; the crystalline calcium silicate hydrate is tobermorite, and the colloidal calcium silicate hydrate is type I CSH gel; in the present invention, the molar ratio of CaO / SiO2 in the crystalline calcium silicate hydrate is preferably 0.83 to 1:1; the molar ratio of CaO / SiO2 in the colloidal calcium silicate hydrate is preferably 1.0 to 1.2:1, more preferably 1.1:1.
[0030] In the present invention, the mass ratio of the crystalline calcium silicate hydrate to the colloidal calcium silicate hydrate is 0.35-0.65:1, preferably 0.35-0.45:1.
[0031] The present invention limits the mass ratio of crystalline calcium silicate hydrate to colloidal calcium silicate hydrate to the above range and can promote C3S and C2S water at the same time; specifically, colloidal calcium silicate hydrate itself can promote C3S hydration, and crystalline calcium silicate hydrate is wrapped by colloidal calcium silicate hydrate to promote C2S hydration. As hydration proceeds, hydration product CSH is generated, and wrapping crystalline calcium silicate hydrate can promote C2S hydration.
[0032] Based on the mass fraction of crystal-colloid mixed hydrated calcium silicate, the ultra-early strength agent provided by the present invention comprises 4 to 10 parts of a reinforcing agent, preferably 5 to 8 parts. In the present invention, the reinforcing agent is preferably diethanol monoisopropanolamine or calcium formate, more preferably diethanol monoisopropanolamine.
[0033] Based on the mass fraction of crystal-colloid mixed hydrated calcium silicate, the ultra-early strength agent provided by the present invention includes 15 to 20 parts of a modifier, preferably 15 to 17 parts. In the present invention, the modifier is preferably potassium sodium tartrate or sodium citrate, more preferably potassium sodium tartrate.
[0034] In the present invention, the reinforcing agent and the modifier are intercalated into the colloidal calcium silicate hydrate, which can double the nucleation sites and thus increase the hydration rate.
[0035] In the present invention, the specific surface area of the ultra-early strengthening agent is preferably 450 to 500 m 2 / kg, more preferably 480 to 500 m 2 / kg.
[0036] The present invention also provides a method for preparing the ultra-early strength agent described in the above technical solution, comprising the following steps:
[0037] dissolving the enhancer and the modifier in water to obtain an auxiliary material solution;
[0038] The auxiliary material solution and α-type calcium silicate hydrate are mixed to carry out a hydrothermal reaction to obtain the super early strength agent; the pressure of the hydrothermal reaction is 0.8-1.2 MPa, the temperature of the hydrothermal reaction is 170-180° C., and the time of the hydrothermal reaction is 4-10 hours.
[0039] The present invention dissolves the enhancer and modifier in water to obtain an auxiliary material solution. In the present invention, the total mass concentration of the enhancer and modifier in the auxiliary material solution is preferably 25-35%, more preferably 30-32%. The present invention has no special requirements for the dissolution, as long as it can be completely dissolved.
[0040] After obtaining the auxiliary material solution, the present invention mixes the auxiliary material solution with α-type calcium silicate hydrate and performs a hydrothermal reaction to obtain the ultra-early strength agent. In the present invention, the preparation method of the α-type calcium silicate hydrate preferably includes the following steps:
[0041] Mixing calcium hydroxide, silicon dioxide and water to obtain a suspension;
[0042] The suspension is subjected to a hydrothermal reaction to obtain the α-type hydrated calcium silicate.
[0043] In the present invention, the molar ratio of calcium hydroxide to silicon dioxide is preferably 1.5 to 1.9:1; more preferably 1.7 to 1.8:1; the water-solid ratio in the suspension is preferably 10. In the present invention, the temperature of the hydrothermal reaction is preferably 190 to 210°C, more preferably 200°C; the time of the hydrothermal reaction is preferably 4.5 to 16.5h, more preferably 16h. In the present invention, the system is preferably cooled to 80°C after the hydrothermal reaction and filtered, and the filtered solid is dried. The present invention has no special requirements for the filtration, and conventional methods in the art can be used. The present invention has no special requirements for the drying, as long as the moisture on the surface of the product can be removed.
[0044] In the present invention, the molar ratio of CaO / SiO2 in the α-type calcium silicate hydrate is preferably 1.5-1.9:1, more preferably 1.7:1.
[0045] In the present invention, the mixing is preferably carried out under stirring conditions, and the stirring speed is preferably 300-800 r / min, more preferably 400-500 r / min; the stirring time is preferably 30-40 min, more preferably 35-40 min.
[0046] In the present invention, the pressure of the hydrothermal reaction is 0.8-1.2 MPa, preferably 0.9-1.0 MPa; the temperature of the hydrothermal reaction is 170-190°C, preferably 180-188°C; the time of the hydrothermal reaction is 4-10 hours, preferably 6-8 hours. In the present invention, the hydrothermal reaction is preferably carried out in an autoclave.
[0047] During the hydrothermal reaction, α-type calcium silicate hydrate is converted into type I CSH gel, and then part of type I CSH gel is converted into crystalline calcium silicate hydrate to obtain crystalline-colloidal mixed calcium silicate hydrate; at the same time, the reinforcing agent and the modifier are intercalated in the type I CSH gel.
[0048] The present invention limits the pressure, temperature and time of the hydrothermal reaction within the above ranges to ensure that a crystalline-colloidal mixed hydrated calcium silicate having a specific mass ratio of crystalline hydrated calcium silicate to colloidal hydrated calcium silicate is obtained.
[0049] In the present invention, the hydrothermal reaction preferably further comprises:
[0050] After the hydrothermal reaction, the system is separated from the solid and the liquid to obtain a solid;
[0051] The solid is dried and then ground to obtain the ultra-early strength agent.
[0052] The present invention has no special requirements for the solid-liquid separation, as long as the solid in the system after the hydrothermal reaction can be separated.
[0053] In the present invention, the drying temperature is preferably 150-200°C, more preferably 160-180°C; the moisture content of the dried product is preferably below 3%, more preferably 1-3%. The present invention has no particular limitation on the drying time, as long as the dried product can reach the above-defined moisture content.
[0054] In the present invention, the average particle size of the ground product is preferably less than 45 μm, more preferably 3 to 12 μm; the specific surface area of the ground product is 450 to 500 m 2 / kg, the present invention has no special limitation on the grinding, as long as the specific surface area of the ground product can meet the above-mentioned limitation requirements.
[0055] In the present invention, the prepared ultra-early strength agent is preferably stored in a silo.
[0056] The present invention also provides the use of the ultra-early strength agent described in the above technical solution or the ultra-early strength agent prepared by the preparation method described in the above technical solution in a cementitious material. In the present invention, the cementitious material preferably includes cement. In the present invention, the mass ratio of the ultra-early strength agent to the cementitious material is preferably 0.3 to 0.6:100, more preferably 0.4 to 05:100.
[0057] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0058] Example 1
[0059] Calcium hydroxide and silicon dioxide in a molar ratio of 1.5:1 are mixed with water to obtain a suspension with a water-solid ratio of 10; the suspension is subjected to a hydrothermal reaction at 200° C. for 16 hours, then cooled to 80° C., filtered, and the filtered solid is dried to obtain an α-type hydrated calcium silicate with a CaO / SiO2 molar ratio of 1.5;
[0060] Dissolve 8 parts of diethanol monoisopropanolamine and 17 parts of potassium sodium tartrate in water to obtain an auxiliary material solution with a total mass concentration of diethanol monoisopropanolamine and potassium sodium tartrate of 30%;
[0061] 75 parts of α-type calcium silicate hydrate with a CaO / SiO2 molar ratio of 1.5 and auxiliary material solution were stirred at a speed of 400r / min for 35min and then transferred to an autoclave for hydrothermal reaction at a pressure of 0.8MPa and a temperature of 170°C for 8h; the solid-liquid separation of the system after the hydrothermal reaction was performed to obtain a solid; the solid was dried at 160°C to a moisture content of 3%; the dried product was ground to obtain an average particle size of 8μm and a specific surface area of 500m 2 / kg of super early strength agent.
[0062] Example 2
[0063] According to the method of Example 1, α-type calcium silicate hydrate was prepared;
[0064] Dissolve 5 parts of diethanol monoisopropanolamine and 15 parts of potassium sodium tartrate in water to obtain an auxiliary material solution with a total mass concentration of diethanol monoisopropanolamine and potassium sodium tartrate of 30%;
[0065] 80 parts of α-type hydrated calcium silicate with a CaO / SiO2 molar ratio of 1.5 and auxiliary material solution were stirred at a speed of 500 r / min for 40 minutes and then transferred to an autoclave for hydrothermal reaction at a pressure of 1.2 MPa and a temperature of 188°C for 6 hours; the solid-liquid separation of the system after the hydrothermal reaction was performed to obtain a solid; the solid was dried at 180°C to a moisture content of 3%; the dried product was ground to obtain an average particle size of 9 μm and a specific surface area of 500 m 2 / kg of super early strength agent.
[0066] Example 3
[0067] The super early strength agent was prepared according to the method of Example 1, except that the α-type calcium silicate hydrate with a CaO / SiO2 molar ratio of 1.5 was replaced by the α-type calcium silicate hydrate with a CaO / SiO2 molar ratio of 1.7; the drying temperature was changed from 160°C to 200°C; the average particle size of the obtained super early strength agent was 8 μm, and the specific surface area was 500 m 2 / kg.
[0068] Example 4
[0069] The super early strength agent was prepared according to the method of Example 2, except that the α-type calcium silicate hydrate with a CaO / SiO2 molar ratio of 1.5 was replaced by the α-type calcium silicate hydrate with a CaO / SiO2 molar ratio of 1.7; the average particle size of the obtained super early strength agent was 9 μm and the specific surface area was 500 m 2 / kg.
[0070] Example 5
[0071] The super early strength agent was prepared according to the method of Example 1, except that the α-type calcium silicate hydrate with a CaO / SiO2 molar ratio of 1.5 was replaced by the α-type calcium silicate hydrate with a CaO / SiO2 molar ratio of 1.9; the average particle size of the obtained super early strength agent was 8 μm and the specific surface area was 500 m 2 / kg.
[0072] Example 6
[0073] The super early strength agent was prepared according to the method of Example 2, except that the α-type calcium silicate hydrate with a CaO / SiO2 molar ratio of 1.5 was replaced by the α-type calcium silicate hydrate with a CaO / SiO2 molar ratio of 1.9; the drying temperature was changed from 180°C to 200°C; the average particle size of the obtained super early strength agent was 9 μm, and the specific surface area was 500 m 2 / kg.
[0074] The ultra-early strength agent prepared in Example 4 was subjected to XRD detection to obtain an XRD spectrum, as shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the characteristic diffraction peak at 2θ of 29° indicates the presence of colloidal calcium silicate hydrate, and the characteristic diffraction peak at 2θ of 7° indicates the presence of crystalline calcium silicate hydrate.
[0075] The ultra-early strength agent prepared in Example 4 was examined by scanning electron microscopy to obtain a SEM image, as shown in FIG. Figure 2 As shown. Figure 2 It can be seen that the super early strength agent provided by the present invention has an intercalation structure.
[0076] The particle size distribution and composition of the ultra-early strength agent prepared in Examples 1 to 6 were tested, and the median particle size was 8 to 9 μm, and the crystal / colloid mass ratio was 0.39 to 0.41, indicating that the composition and particle size of the ultra-early strength agent provided by the present invention meet the cement hydration requirements.
[0077] The super early strength agent prepared in Examples 1 to 6 was added to cement at a super early strength agent to cement mass ratio of 0.3:100 and 0.6:100, respectively, wherein the water-cement ratio of the cement was 0.4; after hydration for 1 day, the hydration resistivity and product content of the cement doped with the super early strength agent were detected, and the results are listed in Table 1; cement without the super early strength agent was used as a comparative example.
[0078] Table 1 Hydration properties of cement after adding super early strength agent
[0079]
[0080]
[0081] It can be seen from Table 1 that adding the ultra-early strength agent prepared in Examples 1 to 6 to cement can significantly improve the 1d resistivity of cement, and increase the 1d hydrated calcium silicate content, ettringite content and calcium hydroxide content of cement, which proves that the ultra-early strength agent provided by the present invention can accelerate the early hydration of cement, promote the coagulation and hardening of cement, and accelerate the formation of hydration products. As the dosage increases, the promotion effect becomes more obvious.
[0082] The super early strength agent prepared in Examples 3 and 4 was added to cement at a mass ratio of 0.3:100 and 0.6:100, respectively, wherein the water-cement ratio of cement was 0.5 and the mortar ratio was 1:3; cement without super early strength agent was used as a comparative example. The prepared mortars were respectively loaded into 40mm×40mm×160mm molds for vibration molding, and the molded specimens were cured for 1 day at 20°C and humidity ≥90%, and demolded; they were continued to be cured at 20°C and humidity ≥90% to 3d, 7d, and 28d ages, and the compressive and flexural strength tests were carried out in accordance with GB / T17671-2021 "Test Method for Cement Mortar Strength (ISO Method)", and the results are listed in Table 2.
[0083] Table 2 Mechanical properties of concrete after adding super early strength agent
[0084]
[0085]
[0086] It can be seen from Table 2 that adding the super early strength agent prepared in Examples 3 and 4 to cement can significantly improve the early strength of cement mortar, with the 1d compressive strength increased by up to 126.86%, and the 1d strength is higher than the 3d strength of the comparative example, and the later strength is also improved to a certain extent.
[0087] The super early strength agent prepared in Example 4 was added into C30 concrete according to the mass ratio of super early strength agent to cement of 0.3:100 and 0.6:100, respectively, with a water-binder ratio of 0.4, a sand ratio of 40%, fly ash replacing 20% of cement, a cementitious material and sand and gravel ratio of 1:4, and after molding, it was placed in a standard curing room and cured to 1d, 3d, 7d, and 28d; concrete without super early strength agent was used as a comparative example; the compressive strength of concrete was tested in accordance with GB / T8076-2008 "Concrete Admixtures", and the results are listed in Table 3.
[0088] Table 3 Mechanical properties of concrete after adding super early strength agent
[0089]
[0090] It can be seen from Table 3 that adding the ultra-early strength agent prepared in Example 4 to concrete will not affect the workability of concrete, and significantly improves the early strength of concrete. The 1d compressive strength is increased by up to 132%, and the 1d compressive strength is higher than the 3d compressive strength of the comparative example, achieving the goal of low dosage and good energy efficiency, and also has a certain promoting effect on the later strength, meeting the strength requirements of C30 concrete.
[0091] The above data prove that the ultra-early strength agent provided by the present invention can simultaneously promote the hydration of C2S and C3S, promote the formation of cement hydration products, greatly improve the early strength of cement under the condition of very low dosage, and promote the later strength, which has broad prospects in engineering applications.
[0092] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. An ultra-early strength agent, comprising the following components in parts by weight: 75-80 parts of crystal-colloidal mixed hydrated calcium silicate; 4-10 parts of enhancer; 15-20 parts of modifier; The crystalline-colloidal mixed calcium silicate hydrate includes crystalline calcium silicate hydrate and colloidal calcium silicate hydrate; the crystalline calcium silicate hydrate is tobermorite, and the colloidal calcium silicate hydrate is type I CSH gel; the mass ratio of the crystalline calcium silicate hydrate to the colloidal calcium silicate hydrate is 0.35-0.65:1; The modifier is sodium potassium tartrate or sodium citrate; The reinforcing agent and the modifier are intercalated in the colloidal hydrated calcium silicate.
2. The ultra-early strength agent according to claim 1, characterized in that: The enhancer is diethanol monoisopropanolamine or calcium formate.
3. The ultra-early strength agent according to claim 1, characterized in that: The molar ratio of CaO / SiO2 in the crystalline hydrated calcium silicate is 0.83-1:
1.
4. The ultra-early strength agent according to claim 1, characterized in that: The molar ratio of CaO / SiO2 in the colloidal calcium silicate hydrate is 1.0-1.2:
1.
5. The ultra-early strengthening agent according to any one of claims 1 to 4, characterized in that: The specific surface area of the super early strength agent is 450-500m 2 / kg.
6. The method for preparing the ultra-early strengthening agent according to any one of claims 1 to 5, comprising the following steps: dissolving the enhancer and the modifier in water to obtain an auxiliary material solution; The auxiliary material solution and α-type calcium silicate hydrate are mixed to carry out a hydrothermal reaction to obtain the super early strength agent; the pressure of the hydrothermal reaction is 0.8-1.2 MPa, the temperature of the hydrothermal reaction is 170-190° C., and the time of the hydrothermal reaction is 4-10 hours.
7. The preparation method according to claim 6, characterized in that: The molar ratio of CaO / SiO2 in the α-type calcium silicate hydrate is 1.5-1.9:
1.
8. Use of the ultra-early strength agent according to any one of claims 1 to 5 or the ultra-early strength agent prepared by the preparation method according to claim 6 or 7 in cementitious materials.
9. The use according to claim 8, characterized in that: The mass ratio of the super early strength agent to the gelling material is 0.3-0.6:100.