A preparation method of iron molybdate and its application in photocatalytic degradation of pollutants in water

By using the hydrothermal reaction and sintering technology of MIL-88 (Fe-MOF) and ammonium molybdate tetrahydrate in the preparation process of Fe2(MoO4)3, the problem of Fe2(MoO4)3 without doping or heterojunction is solved The problem of high-efficiency photocatalytic degradation performance is achieved, and efficient degradation of pollutants in water is achieved, especially the degradation rate of tetracycline hydrochloride is significantly improved.

CN116375095BActive Publication Date: 2024-10-22ZHEJIANG XINGUANG PHARM CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310388631.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-22
Estimated Expiration
2043-04-13

AI Technical Summary

Technical Problem

At present, the high-performance application of Fe2(MoO4)3 as a photocatalyst is limited, mainly because it requires doping or construction of heterojunctions to achieve efficient degradation performance. There is a lack of methods to achieve efficient photocatalysis without these means.

Method used

Iron molybdate is prepared by hydrothermal reaction between MIL-88 (Fe-MOF) and ammonium molybdate tetrahydrate under specific conditions, followed by ultrasonic treatment and pH adjustment, and finally sintering at high temperature to produce Fe2(MoO4)3 , achieving its high photocatalytic degradation performance.

Benefits of technology

This method allows Fe2(MoO4)3 to significantly improve its degradation efficiency of pollutants in water without the need for doping or construction of heterojunctions. For example, the degradation rate of tetracycline hydrochloride reaches 85-90%, which is better than traditional FeCl3 ·6H2O is iron molybdate synthesized from iron source.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116375095B_ABST
    Figure CN116375095B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of ferric molybdate and its application in photocatalytic degradation of pollutants in water, comprising the following steps: S1: taking an appropriate amount of MIL-88 (Fe-MOF) and an appropriate amount of water and putting them into a 100ml reactor, stirring at a medium speed for 10 minutes at room temperature to obtain a Fe-MOF solution; S2: taking an appropriate amount of ammonium molybdate tetrahydrate and water and putting them into a small beaker, stirring for 10 minutes, and obtaining an ammonium molybdate solution; S3: after completing the stirring, respectively stirring the Fe-MOF solution and the molybdenum tetrahydrate; S4: slowly drip the ammonium molybdate solution into the Fe-MOF solution, adjust the pH with nitric acid, and stir at room temperature for one hour; S5: put the reactor into a 120-200℃ drying oven for hydrothermal reaction for 6-48h; S6: after the reaction is completed, cool to room temperature, wash with water and ethanol alternately three times to obtain the iron molybdate material; S7: burn the iron molybdate material in a muffle furnace or a tube furnace for 30-120min to obtain Fe2(MoO4)3. Fe2(MoO4)3 derived from MOF can be used to efficiently decompose tetracycline hydrochloride in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of new materials, and in particular to a method for preparing ferric molybdate and application of the same in photocatalytically degrading pollutants in water. Background Art

[0002] Iron molybdate (Fe2(MoO4)3) has attracted the attention of researchers due to its thermal stability, chemical stability, low cost and excellent redox performance. Fe2(MoO4)3 has a band gap of 2.7eV and has great potential as a photocatalyst. Fe2(MoO4)3 has good pollutant degradation performance, but it is not a high-performance photocatalyst. In recent reports, Fe2(MoO4)3 is more used to construct heterojunctions with other semiconductors to exert photocatalytic effects. How to make Fe2(MoO4)3 have high photocatalytic degradation performance without doping or constructing heterojunctions is a problem that needs to be solved at this stage. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing iron molybdate and its application in photocatalytic degradation of pollutants in water, which has the advantage of enabling Fe2(MoO4)3 to have high photocatalytic degradation performance without doping or constructing a heterojunction.

[0004] The above technical objectives of the present invention are achieved through the following technical solutions:

[0005] A method for preparing iron molybdate, characterized in that it comprises the following steps:

[0006] S1: Take an appropriate amount of MIL-88 (Fe-MOF) and an appropriate amount of water and put them into a 100 ml reactor. Stir at a medium speed for 10 minutes at room temperature to prepare a Fe-MOF solution.

[0007] S2: Put an appropriate amount of ammonium molybdate tetrahydrate and water into a small beaker and stir for 10 minutes to prepare an ammonium molybdate solution;

[0008] S3: After the stirring in S1 and S2 is completed, the Fe-MOF solution and the ammonium molybdate solution are ultrasonicated for 10 minutes respectively;

[0009] S4: slowly drip the ammonium molybdate solution into the Fe-MOF solution, adjust the pH with nitric acid, and stir at room temperature for one hour;

[0010] S5: Place the reactor in a drying oven at 120-200°C for hydrothermal reaction for 6-48 hours;

[0011] S6: After the reaction is completed, the mixture is cooled to room temperature and washed alternately with water and ethanol three times to obtain an iron molybdate material;

[0012] S7: Burn the iron molybdate material in a muffle furnace or a tube furnace for 30-120 minutes to obtain Fe2(MoO4)3.

[0013] Preferably, the mass of MIL-88 (Fe-MOF) in S1 is 0.2629 g, and the volume of water is 30 ml; the mass of ammonium molybdate tetrahydrate in S2 is 0.3972 g, and the volume of water is 30 ml.

[0014] Preferably, the pH value in S4 is adjusted within the range of 1-4.

[0015] Preferably, the temperature during sintering in the muffle furnace or tubular furnace in S7 is 500-600° C., and the heating rate is 0.5-10° C. / min.

[0016] Preferably, the Fe2(MoO4)3 is used to degrade tetracycline hydrochloride in water.

[0017] The beneficial effects of the present invention are: using MOF as a precursor or sacrificial template to synthesize new MOF derivatives not only inherits many advantages of the MOF material itself, but also retains the parent morphology. Using Fe-MOF as an iron source, the synthesis of iron molybdate has better photocatalytic degradation performance than using traditional FeCl3·6H2O. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is the XRD pattern of Fe2(MoO4)3 derived from MOF in Example;

[0019] Figure 2 This is the SEM image of Fe2(MoO4)3 derived from MOF in the example. DETAILED DESCRIPTION

[0020] The following is only a preferred embodiment of the present invention, and the protection scope is not limited to this embodiment. All technical solutions under the concept of the present invention should belong to the protection scope of the present invention. The same parts are represented by the same reference numerals.

[0021] Example 1: Preparation of Fe2(MoO4)3 derived from MOF: Weigh 0.2629 g of MIL-88 and 30 ml of water into a 100 ml reactor and stir at medium speed for 10 minutes at room temperature; weigh 0.3972 g of ammonium molybdate tetrahydrate and 30 ml of water into a small beaker and stir for 10 minutes. After the solid is stirred, ultrasonicate for 10 minutes. After that, slowly drip the ammonium molybdate solution into the MIL-88 solution and adjust the pH to about 3.4 with nitric acid. Stir at room temperature for one hour, and put the reactor into a 170°C drying oven for hydrothermal reaction for 15 hours. After the reaction is completed, cool to room temperature, wash with water and ethanol alternately three times, dry, and burn at 550°C in a tube furnace for 30 minutes, with a heating rate of 5°C / min.

[0022] Preparation of iron molybdate synthesized with FeCl3·6H2O as the iron source: replace the above MIL-88 with FeCl3·6H2O, and keep other conditions unchanged.

[0023] Photocatalytic degradation test: 50 mg Fe2(MoO4)3 was dispersed in 80 mL tetracycline hydrochloride (20 mg / L) aqueous solution. After irradiation with visible light for 3 h, MOF-derived Fe2(MoO4)3 could degrade 85% of tetracycline hydrochloride, while iron molybdate synthesized with FeCl3·6H2O as the iron source could only degrade 49% of tetracycline hydrochloride.

[0024] Example 2: Preparation of Fe2(MoO4)3 derived from MOF: Weigh 0.2629 g of MIL-88 and 30 ml of water into a 100 ml reactor and stir at medium speed for 10 minutes at room temperature; weigh 0.3972 g of ammonium molybdate tetrahydrate and 30 ml of water into a small beaker and stir for 10 minutes. After the solid is stirred, ultrasonicate for 10 minutes. After that, slowly drip the ammonium molybdate solution into the MIL-88 solution and adjust the pH to about 3.3 with nitric acid. Stir at room temperature for one hour, and put the reactor into a 170°C drying oven for hydrothermal reaction for 12 hours. After the reaction is completed, cool to room temperature, wash with water and ethanol alternately three times, dry, and burn at 550°C in a tube furnace for 30 minutes, with a heating rate of 0.5°C / min.

[0025] Preparation of iron molybdate synthesized with FeCl3·6H2O as the iron source: replace the above MIL-88 with FeCl3·6H2O, and keep other conditions unchanged.

[0026] Photocatalytic degradation test: 50 mg Fe2(MoO4)3 was dispersed in 80 mL tetracycline hydrochloride (20 mg / L) aqueous solution. After irradiation with visible light for 3 h, MOF-derived Fe2(MoO4)3 could degrade 90% of tetracycline hydrochloride, while iron molybdate synthesized with FeCl3·6H2O as the iron source could only degrade 51% of tetracycline hydrochloride.

[0027] The specific embodiments described above further illustrate the technical problems, technical solutions and beneficial effects solved by the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing iron molybdate, characterized in that: The following steps are involved: S1: Take an appropriate amount of Fe-MOF and an appropriate amount of water and put them into a 100 mL reactor, wherein the Fe-MOF is MIL-88, and stir at a medium speed for 10 minutes at room temperature to obtain a Fe-MOF solution; S2: Put an appropriate amount of ammonium molybdate tetrahydrate and water into a small beaker and stir for 10 minutes to prepare an ammonium molybdate solution; S3: After the stirring in S1 and S2 is completed, the Fe-MOF solution and the ammonium molybdate solution are ultrasonicated for 10 minutes respectively; S4: slowly drip the ammonium molybdate solution into the Fe-MOF solution, adjust the pH value with nitric acid, and stir at room temperature for one hour; S5: Place the reactor in a drying oven at 120-200°C for hydrothermal reaction for 6-48 hours; S6: After the reaction is completed, the mixture is cooled to room temperature and washed alternately with water and ethanol three times to obtain an iron molybdate material; S7: calcining the iron molybdate material in a muffle furnace or a tube furnace for 30-120 minutes to obtain Fe2(MoO4)3.

2. The method for preparing ferric molybdate according to claim 1, wherein The mass of MIL-88 described in S1 is 0.2629 g, and the volume of water is 30 mL; the mass of ammonium molybdate tetrahydrate described in S2 is 0.3972 g, and the volume of water is 30 mL.

3. The method for preparing ferric molybdate according to claim 1, wherein: The pH value in S4 was adjusted in the range of 1-4.

4. The method for preparing ferric molybdate according to claim 1, wherein The temperature during sintering in the muffle furnace or tubular furnace in S7 is 500-600° C., and the heating rate is 0.5-10° C. / min.

5. Application of iron molybdate prepared by the preparation method according to any one of claims 1 to 4 in photocatalytic degradation of pollutants in water, characterized in that: The Fe2(MoO4)3 is used to degrade tetracycline hydrochloride in water.

Citation Information

Cited By

  • A heteropoly acid metal organic framework compound and a synthesis method and application thereof