Coating, preparation and treatment method for improving surface accuracy of layered extrusion-formed ceramics
By using coatings composed of refractory aggregates and other materials on the surface of layered extruded ceramics and performing high-temperature baking treatment, the problem of difficulty in improving the surface accuracy of ceramic core/shell is solved, and the significant reduction in surface roughness and thermal stability of ceramics are achieved. Improved, suitable for the production of complex ceramic parts.
Patent Information
- Application Number
- CN202310059120.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-01-18
AI Technical Summary
The surface accuracy of ceramic core/shell formed by layered extrusion is difficult to meet the requirements of investment casting, mainly due to the layering effect that makes it difficult to reduce the surface roughness. Existing methods cannot meet the accuracy requirements of complex-structured ceramic parts.
A coating including refractory aggregates, binders, suspending agents, pore-forming agents and thickeners is used. The coating is evenly adsorbed on the ceramic surface through dipping, brushing or centrifugal methods, and is roasted at high temperatures to reduce Surface roughness.
It effectively reduces the surface roughness of layered extrusion-formed ceramics to Ra below 6.3μm, improves the surface accuracy of ceramic core/shell, has good thermal stability and cost-effectiveness, and is suitable for the production of complex ceramic parts.
Smart Images

Figure CN116375492B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field related to rapid casting, and more specifically, relates to a coating for improving the surface accuracy of layered extrusion-formed ceramics, and a preparation and treatment method thereof. Background Art
[0002] With the rapid development of the aerospace industry, the structures of new generation engines, hydraulic valve bodies and other castings are developing towards integration, hollow thin-wall and complexity in order to improve the precision of castings and reduce their weight. The traditional ceramic core / shell preparation methods are mainly gel injection molding, injection molding or hot pressing molding. These traditional preparation methods require mold molding and are easily limited by the structure of the core. At the same time, the material system used contains more organic matter, which will cause certain harm and pollution to the human body and the environment during the production process, and does not meet the current green and environmentally friendly production requirements.
[0003] Since the advent of additive manufacturing technology in the 1990s, it has significantly shortened the development time of new products and reduced development costs. Additive manufacturing provides a new method for the rapid preparation of ceramic cores / shells. At present, the main additive manufacturing methods for ceramics include micro-injection bonding forming, layered micro-extrusion forming, selective laser sintering forming, photocuring forming, etc. Compared with several other additive manufacturing methods, the advantage of layered extrusion forming ceramic shells is that there is no need to introduce ultraviolet light or laser irradiation, the slurry has a high solid content and small sintering shrinkage, and the equipment of layered extrusion forming itself is simple, easy to maintain, and the cost of construction and use is very low. In addition, most of the slurry systems used in layered extrusion forming are non-toxic and harmless and have low cost. Specifically, for example, CN105599106A discloses a micro-injection bonding forming method for a ceramic core blank, first laying a powder matrix material, and then using a nozzle to spray a binder in a selected area, and finally forming the required ceramic core blank. This spray bonding equipment has a high cost, the porosity of the core blank is large, and the surface accuracy does not meet the requirements of investment casting (Ra <6.3μm). For example, CN110228996A discloses a method for preparing a ceramic core based on slurry direct writing, and the obtained ceramic core has suitable mechanical properties and high dimensional accuracy, but there is no specific description of the surface accuracy. Due to the inherent characteristics of the layered extrusion forming process (layer effect), the existing method mainly improves the surface roughness of the layered extrusion formed ceramic sample by optimizing the process, but its surface roughness is still difficult to reach below 12.5μm, and there are still few coating materials suitable for improving the surface accuracy of extrusion formed ceramics.
[0004] Compared with the traditional ceramic core / shell preparation method, although layered extrusion can quickly form ceramic parts with more complex structures without molds, it has many advantages such as short production cycle, low overall cost, and flexible processing. However, due to the layer effect, the surface accuracy of the ceramic core / shell prepared by layered extrusion is low, and it is currently difficult to meet the requirements of investment casting (Ra < 6.3μm), which is also a key issue restricting its development. Therefore, this field urgently needs to find a more complete solution to meet the accuracy requirements of the rapid preparation of ceramic core / shell and other parts. Summary of the invention
[0005] In view of the above defects or improvement needs of the prior art, the present invention provides a coating, preparation and treatment method for improving the surface accuracy of layered extrusion-formed ceramics, thereby solving the problem that it is difficult to improve the surface accuracy of layered extrusion-formed ceramic blanks.
[0006] To achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a coating for improving the surface accuracy of layered extrusion-formed ceramics, the coating comprising 30 to 50 parts of refractory aggregate, 10 to 25 parts of binder, 4 to 10 parts of suspending agent and pore-forming agent, 10 to 25 parts of thickener, and the rest being a carrier liquid.
[0007] Further preferably, the refractory aggregate is alumina and silica ceramic powder with a particle size of 800-1500 mesh.
[0008] More preferably, the binder is a polyvinyl pyrrolidone aqueous solution with a solubility of 10% to 30%.
[0009] More preferably, the suspending agent and pore-forming agent are calcium carbonate powder with a particle size of 800-1500 mesh.
[0010] Further preferably, the thickener is a bentonite aqueous solution with a mass fraction of 5% to 25%, and the particle size of the bentonite is 1000 mesh to 1500 mesh.
[0011] According to another aspect of the present invention, a method for preparing the above-mentioned coating is provided, characterized in that the method comprises mixing the refractory aggregate, binder, suspending agent with pore-forming agent, thickener and carrier liquid, and ball milling them uniformly to obtain the desired coating.
[0012] According to another aspect of the present invention, there is provided a method for treating the surface of a layered extrusion-formed ceramic using the coating described above, characterized in that the treatment method comprises the following steps:
[0013] S1: applying the coating on the surface of the ceramic to be treated by dipping, brushing or centrifugation, leaving it to stand and drying;
[0014] S2 is to integrally sinter the ceramic to be processed after step S1, and obtain the required high surface precision ceramic after cooling.
[0015] Further preferably, in step S1, in the dipping, brushing or centrifugal method, the contact time between the coating and the ceramic to be treated is 2s to 20s, and the coating thickness is 0.1mm to 0.5mm.
[0016] Further preferably, in step S1, the drying method is natural drying in the shade, and the drying time is 2 hours to 6 hours.
[0017] Further preferably, in step S2, the temperature of the debinding stage in the roasting is 300°C to 500°C, and the holding time is 0.5h to 4h; the sintering temperature is 1000°C to 1600°C, and the holding time is 0.5h to 2h; the heating rate during the sintering process is 2°C / min to 5°C / min.
[0018] In general, the above technical solutions conceived by the present invention have the following beneficial effects compared with the prior art:
[0019] 1. The present invention proposes a surface coating for layered extrusion-formed ceramic core / shell through pioneering research, and designs the coating composition and coating process to achieve uniform and smooth adsorption of the coating on the surface of the ceramic body, so that the surface roughness Ra of the ceramic part formed by layered micro-extrusion is reduced from 12.5 to 30 μm to below 6.3 μm, solving the problem that it is difficult to improve the surface accuracy of the ceramic body formed by layered extrusion;
[0020] 2. The surface coating provided by the present invention can withstand a high temperature of 1600°C and has better thermal stability than conventional ceramic coatings on the market. The ceramic core / shell can maintain a high surface accuracy at different sintering temperatures;
[0021] 3. The chemical composition of the coating of the present invention is clear, and the proportion of the corresponding components can be adjusted in a targeted manner according to different use requirements (such as temperature tolerance, coating thickness, air permeability, etc.). The entire coating system has good flexibility and controllability, and can be adapted to various materials of complex ceramic core / shell and other parts, and the coating can be closely combined with the substrate;
[0022] 4. The material system of the coating of the present invention has the advantages of low cost and green environmental protection, simple coating process and short cycle, and is suitable for actual production. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a flow chart of a coating treatment method for layered extrusion-formed ceramics constructed according to a preferred embodiment of the present invention;
[0024] Figure 21 is a schematic diagram of a before-and-after comparison of a ceramic coating based on layered extrusion molding constructed according to a preferred embodiment of the present invention, wherein (a) is a coating applied to a curved substrate, and (b) is a coating applied to a straight substrate;
[0025] Figure 3 is a diagram showing the effect of the coating constructed according to the preferred embodiment of the present invention on improving the ceramic precision;
[0026] Figure 4 It is a comparative data diagram of thermal stability between ordinary ceramic coating and the present coating constructed according to the preferred embodiment of the present invention;
[0027] Figure 5 It is a surface microscopic topography of the coating and the ceramic substrate constructed according to the preferred embodiment of the present invention;
[0028] Figure 6 It is a microscopic morphology of the fracture surface of the coating and the ceramic substrate constructed according to the preferred embodiment of the present invention;
[0029] Figure 7 It is a physical effect diagram constructed according to the preferred embodiment of the present invention and used to demonstrate the effect of coating on improving the surface precision of ceramics. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0031] A coating for improving layered extrusion forming ceramics, the new coating material composition and important proportions are 30-50 parts of refractory aggregate, 10-25 parts of binder, 4-10 parts of suspending agent and pore-forming agent, 10-25 parts of thickener, and 25-40 parts of carrier liquid.
[0032] The refractory aggregate is alumina and silica ceramic powder with a particle size of 800-1500 mesh. The refractory temperature of alumina powder can reach above 1800°C. It can maintain a stable shape during calcination, thus acting as a network intermediate of the coating. In addition, when the coating is calcined at high temperature, the silica particles will partially melt, which can not only penetrate into the gaps between alumina particles to improve the strength of the coating itself, but also achieve a close combination of the coating and the ceramic shell substrate.
[0033] The binder is a polyvinyl pyrrolidone aqueous solution with a solubility of 10% to 30%. As a synthetic water-soluble polymer compound, polyvinyl pyrrolidone does not react with other components in the coating and has excellent solubility, film-forming property and adhesion. The addition of polyvinyl pyrrolidone can enhance the wetting effect of the coating and facilitate the coating.
[0034] The suspending agent and pore-forming agent are calcium carbonate powder with a particle size of 800-1500 mesh. The selected calcium carbonate powder can not only improve the suspension stability of the coating, but also decompose and produce gas during the high-temperature roasting stage, thereby forming tiny holes in the coating and improving the air permeability of the coating;
[0035] The thickener is a bentonite aqueous solution with a mass fraction of 5% to 25%. The particle size of the bentonite is 1000 to 1500 meshes. The bentonite can be dispersed into a gel and a suspension in an aqueous medium. Its aqueous solution has a certain viscosity and thixotropy, which helps the coating to be quickly fixed after being adsorbed to the surface of the substrate, so that the thickness of the coating is uniform everywhere. The carrier liquid is water.
[0036] As a further preference, the ceramic coating should have excellent leveling properties and good wettability with the surface of the layered extruded ceramic core / shell.
[0037] As a further preferred embodiment, the ceramic core / shell is formed by layered extrusion, and the ceramic core / shell matrix material includes aluminum oxide, zirconium oxide, silicon oxide, and yttrium oxide ceramics.
[0038] like Figure 1 As shown, the method steps of treating the ceramic to be treated with the above coating include:
[0039] S1 uses dipping, brushing or centrifugal methods to apply the coating on the surface of the layered extrusion-molded ceramic core / shell, and controls the contact time between the coating and the ceramic core / shell to adjust the thickness of the ceramic coating;
[0040] S2 allows the ceramic core / shell with a coating of a certain thickness to stand and dry in a natural environment;
[0041] S3 integrally bakes the ceramic core / shell and the coating, and obtains a ceramic core / shell with high surface precision after cooling.
[0042] As a further preferred embodiment, in S1, the contact time between the coating and the ceramic is 2 to 20 seconds, and the coating thickness can be controlled to be 0.1 to 0.5 mm according to the coating time; the surface coating is dried naturally in the shade for 2 to 6 hours.
[0043] As a further preference, the sintering process includes a degreasing stage and a sintering stage, wherein the temperature of the degreasing stage is 300-500°C, and the holding time is 0.5-4h; the temperature of the sintering stage is 1000-1600°C, and the holding time is 0.5-2h; the heating rate of the coating and ceramic core / shell matrix during the sintering process is 2-5°C / min.
[0044] like Figure 2 As shown, by applying the coating, the layered undulations on the surface of the ceramic substrate can be significantly eliminated, wherein (a) is a comparison of the ceramic substrate before and after the coating when the ceramic substrate is a curved surface, and (b) is a comparison of the ceramic substrate before and after the coating when the ceramic substrate is a straight surface.
[0045] like Figure 3 As shown in the figure, the experimental data show that the coating greatly improves the surface accuracy of samples with different inclination angles. From 15° to 90°, the surface roughness gradually decreases. Compared with the sample without coating, the surface accuracy of the sample after coating can be improved by 3 to 6 times. When the inclination angle is 90°, the surface roughness of the ceramic substrate can reach 3.6μm at best.
[0046] like Figure 4 As shown in the figure, ordinary ceramic coatings can only maintain stable performance below 1200℃. When the temperature rises to 1300℃ or higher, the coating will show obvious component burnout and layer thickness reduction, resulting in the inability to completely cover the layer undulations on the surface of the ceramic substrate. The coating developed by this patent can withstand higher temperatures and can still maintain stable layer thickness and strength after being kept at 1500℃ for 30 minutes, which can effectively improve the surface accuracy of the ceramic substrate.
[0047] like Figure 5 As shown, the surface microstructure of the coating and the ceramic substrate is demonstrated. The left side is the layered surface of the ceramic substrate, and the right side is the relatively smooth surface of the sample after the coating is applied.
[0048] like Figure 6 As shown, the cross-sectional microstructure of the combination of the coating and the ceramic substrate is displayed. The wavy dotted line marked in the middle is the boundary between the ceramic substrate and the coating. It can be seen that the coating has achieved the effect of combining with the substrate and covering the undulating layers on the substrate surface.
[0049] like Figure 7 The figure shows the actual effect of applying coating to the ceramic sample. Figure (a) shows the sample without coating, and Figure (b) shows the sample after coating. By comparing the two, it can be seen that the coating has greatly eliminated the layer effect on the surface of the ceramic sample.
[0050] The present invention will be further described below with reference to specific embodiments.
[0051] Embodiment 1:
[0052] (1) The required alumina-based ceramic core blank is prepared by layered micro-extrusion forming technology, and the surface roughness of the blank after drying and sintering is 19 μm.
[0053] (2) Alumina powder (800 mesh), silica powder (800 mesh), calcium carbonate powder (800 mesh), 10% by mass lithium bentonite (1000 mesh) aqueous solution, 10% by mass PVP aqueous solution, and water are mixed and ball-milled to obtain a coating. The coating includes 15 parts of alumina powder and 15 parts of silica powder, 30 parts of refractory aggregate, 5 parts of calcium carbonate powder as suspending agent and pore-forming agent, 15 parts of lithium bentonite aqueous solution as thickener, 20 parts of PVP aqueous solution as binder, and 30 parts of carrier water.
[0054] (3) Immerse the ceramic core in the coating for 10 seconds, take it out and fix it with a clamp.
[0055] (4) The coated ceramic core blank was placed in a ventilated place to dry naturally for 2 hours at an ambient temperature of 25°C. The coating thickness was 0.3 mm.
[0056] (5) The dried coated body is dehydrated, degreased and sintered. The heating rate during the sintering process is 2°C / min. The temperature of the degreasing stage is 300°C, and the holding time is 0.5 h. The temperature of the sintering stage is 1000°C, and the holding time is 0.5 h. After cooling, a ceramic core sample with high surface accuracy is obtained, and the surface roughness is 4.1 μm.
[0057] Embodiment 2:
[0058] (1) The required zirconia-based ceramic core blank is prepared by layered micro-extrusion forming technology, and the surface roughness of the blank after drying and sintering is 16 μm.
[0059] (2) Alumina powder (1500 mesh), silica powder (1500 mesh), calcium carbonate powder (1250 mesh), 5% sodium bentonite (1250 mesh) aqueous solution, 10% PVP aqueous solution, and water are mixed and ball-milled to obtain a coating. The coating includes 25 parts of alumina powder and 25 parts of silica powder, 50 parts of refractory aggregate, 4 parts of calcium carbonate powder as suspending agent and pore-forming agent, 10 parts of sodium bentonite aqueous solution as thickener, 10 parts of PVP aqueous solution as binder, and 26 parts of carrier water.
[0060] (3) Immerse the ceramic core in the coating for 5 seconds, take it out and fix it with a clamp.
[0061] (4) The coated ceramic core blank was placed in a ventilated place to dry naturally for 4 hours at an ambient temperature of 20°C. The coating thickness was 0.2 mm.
[0062] (5) The dried coated body is dehydrated, degreased and sintered. The heating rate during the sintering process is 3°C / min. The temperature of the degreasing stage is 400°C and the holding time is 1h. The temperature of the sintering stage is 1100°C and the holding time is 1h. After cooling, a ceramic core sample with high surface accuracy is obtained, and the surface roughness is 4.2μm.
[0063] Embodiment 3:
[0064] (1) The required silicon oxide-based ceramic core blank is prepared by layered micro-extrusion forming technology, and the surface roughness of the blank is 30 μm after drying and sintering.
[0065] (2) Alumina powder (800 mesh), silica powder (1000 mesh), calcium carbonate powder (1500 mesh), 5% calcium-based bentonite (1250 mesh) aqueous solution, 10% PVP aqueous solution, and water are mixed and ball-milled to obtain a coating. The coating includes 15 parts of alumina powder and 20 parts of silica powder, 35 parts of refractory aggregate, 5 parts of calcium carbonate powder as a suspending agent and pore-forming agent, 10 parts of calcium-based bentonite aqueous solution as a thickener, 20 parts of PVP aqueous solution as a binder, and 30 parts of carrier water.
[0066] (3) Immerse the ceramic core in the coating for 2 seconds, take it out and fix it with a clamp.
[0067] (4) The coated ceramic core blank was placed in a ventilated place to dry naturally for 4 hours at an ambient temperature of 20°C. The coating thickness was 0.1 mm.
[0068] (5) The dried coated body is dehydrated, degreased and sintered. The heating rate during the sintering process is 4°C / min, the temperature of the degreasing stage is 500°C, the holding time is 1h, the temperature of the sintering stage is 1200°C, and the holding time is 1h. After cooling, a ceramic core sample with high surface accuracy is obtained, and the surface roughness is 6.0μm.
[0069] Embodiment 4:
[0070] (1) The required yttria-based ceramic core blank is prepared by layered micro-extrusion forming technology, and the surface roughness of the blank after drying and sintering is 14 μm.
[0071] (2) Alumina powder (1250 mesh), silica powder (800 mesh), calcium carbonate powder (1250 mesh), 5% by mass lithium bentonite (1500 mesh) aqueous solution, 10% by mass PVP aqueous solution, and water are mixed and ball-milled to obtain a coating, wherein the coating comprises 20 parts of alumina powder and 10 parts of silica powder, 30 parts of refractory aggregate in total; 5 parts of calcium carbonate powder as a suspending agent and pore-forming agent; 15 parts of lithium bentonite aqueous solution as a thickener; 10 parts of PVP aqueous solution as a binder; and 40 parts of carrier water.
[0072] (3) Immerse the ceramic core in the coating for 20 seconds, take it out and fix it with a clamp.
[0073] (4) The coated ceramic core blank was placed in a ventilated place to dry naturally for 6 hours at an ambient temperature of 25°C and a coating thickness of 0.5 mm.
[0074] (5) The dried coated body is dehydrated, degreased and sintered. The heating rate during the sintering process is 5°C / min, the temperature of the degreasing stage is 500°C, the holding time is 2h, the temperature of the sintering stage is 1300°C, the holding time is 1h, and after cooling, a ceramic core sample with high surface accuracy is obtained, and the surface roughness is 3.6μm.
[0075] Embodiment 5:
[0076] (1) The required zirconia-based ceramic shell body is prepared by layered micro-extrusion forming technology, and the surface roughness of the body after drying and sintering is 20 μm.
[0077] (2) Alumina powder (1000 mesh), silica powder (1000 mesh), calcium carbonate powder (1000 mesh), 20% sodium bentonite (1000 mesh) aqueous solution, 20% PVP aqueous solution, and water are mixed and ball-milled to obtain a coating. The coating includes 10 parts of alumina powder and 20 parts of silica powder, 30 parts of refractory aggregate, 10 parts of calcium carbonate powder as suspending agent and pore-forming agent, 25 parts of sodium bentonite aqueous solution as thickener, 10 parts of PVP aqueous solution as binder, and 25 parts of carrier water.
[0078] (3) Immerse the ceramic shell in the coating for 4 seconds, take it out and fix it with a clamp.
[0079] (4) The coated ceramic shell body was placed in a ventilated place to dry naturally for 2 hours at an ambient temperature of 20°C. The coating thickness was 0.2 mm.
[0080] (5) The dried coated body is dehydrated, degreased and sintered. The heating rate during the sintering process is 4°C / min, the temperature of the degreasing stage is 400°C, the holding time is 1h, the temperature of the sintering stage is 1400°C, and the holding time is 1h. After cooling, a ceramic shell specimen with high surface accuracy is obtained, and the surface roughness is 4.6μm.
[0081] Embodiment 6:
[0082] (1) The required alumina-based ceramic shell body is prepared by layered micro-extrusion forming technology, and the surface roughness of the body after drying and sintering is 28 μm.
[0083] (2) Alumina powder (1250 mesh), silica powder (1250 mesh), calcium carbonate powder (1500 mesh), 15% by mass calcium-based bentonite (1500 mesh) aqueous solution, 30% by mass PVP aqueous solution, and water are mixed and ball-milled to obtain a coating. The coating includes 20 parts of alumina powder and 15 parts of silica powder, 35 parts of refractory aggregate, 8 parts of calcium carbonate powder as a suspending agent and pore-forming agent, 20 parts of calcium-based bentonite aqueous solution as a thickener, 12 parts of PVP aqueous solution as a binder, and 25 parts of carrier water.
[0084] (3) Immerse the ceramic shell in the coating for 15 seconds, take it out and fix it with a clamp.
[0085] (4) The coated ceramic shell body was placed in a ventilated place to dry naturally for 4 hours at an ambient temperature of 25°C. The coating thickness was 0.4 mm.
[0086] (5) The dried coating body is dehydrated, degreased and sintered. The heating rate during the sintering process is 3°C / min, the temperature of the degreasing stage is 300°C, the holding time is 1.5h, the temperature of the sintering stage is 1500°C, and the holding time is 0.5h. After cooling, a ceramic shell specimen with high surface accuracy is obtained, and the surface roughness is 5.1μm.
[0087] Embodiment 7:
[0088] (1) The required alumina-based ceramic core blank is prepared by layered micro-extrusion forming technology, and the surface roughness of the blank after drying and sintering is 24 μm.
[0089] (2) Alumina powder (1000 mesh), silica powder (800 mesh), calcium carbonate powder (800 mesh), 25% by mass lithium bentonite (1250 mesh) aqueous solution, 15% by mass PVP aqueous solution, and water are mixed and ball-milled to obtain a coating. The coating includes 15 parts of alumina powder and 15 parts of silica powder, 30 parts of refractory aggregate, 8 parts of calcium carbonate powder as a suspending agent and pore-forming agent, 12 parts of lithium bentonite aqueous solution as a thickener, 25 parts of PVP aqueous solution as a binder, and 25 parts of carrier water.
[0090] (3) Immerse the ceramic core in the coating for 8 seconds, take it out and fix it with a clamp.
[0091] (4) The coated ceramic core blank was placed in a ventilated place to dry naturally for 6 hours at an ambient temperature of 20°C. The coating thickness was 0.3 mm.
[0092] (5) The dried coated body is dehydrated, degreased and sintered. The heating rate during the sintering process is 2°C / min. The temperature of the degreasing stage is 400°C and the holding time is 4 h. The temperature of the sintering stage is 1600°C and the holding time is 2 h. After cooling, a ceramic core sample with high surface accuracy is obtained, and the surface roughness is 4.7 μm.
[0093] In summary, the surface coating material and use method for layered extrusion forming of ceramic cores / shells proposed in the present invention can greatly improve the surface accuracy of ceramic parts, and the coating system has the advantages of low cost, green environmental protection, high temperature resistance, flexible use and strong controllability. At the same time, the coating process is simple and the processing cycle is short. It is particularly suitable for the production of complex ceramic cores / shells and other parts. This method can promote the practical application of related rapid prototyping technologies in the field of precision casting, improve the manufacturing level of the casting industry, and has important theoretical and practical significance.
[0094] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for treating the surface of layered extruded ceramics with a coating that improves the surface accuracy of layered extruded ceramics, It is characterized in that The processing method comprises the following steps: S1: Apply the coating on the ceramic surface to be treated by dipping, brushing or centrifugal method, let it stand and dry; S2: calcining the ceramic to be processed after step S1 as a whole, and obtaining the required high surface precision ceramic after cooling, wherein the surface roughness of the ceramic is less than 6.3 μm; The coating comprises 30-50 parts of refractory aggregate, 10-25 parts of binder, 4-10 parts of suspending agent and pore-forming agent, 10-25 parts of thickener, and the rest is carrier liquid; The refractory aggregate is alumina and silicon oxide ceramic powder, and the particle size is 800 mesh to 1500 mesh; The binder is a polyvinyl pyrrolidone aqueous solution with a solubility of 10% to 30%; The suspending agent and pore-forming agent are calcium carbonate powder with a particle size of 800-1500 mesh; The thickener is a bentonite aqueous solution with a mass fraction of 5% to 25%, and the particle size of the bentonite is 1000 mesh to 1500 mesh; In step S1, in the dipping, brushing or centrifugal method, the contact time between the coating and the ceramic to be treated is 2s to 20s, and the coating thickness is 0.1mm to 0.5mm; In step S2, the temperature of the debinding stage in the roasting is 300°C to 500°C, and the holding time is 0.5h to 4h; the sintering temperature is 1000°C to 1600°C, and the holding time is 0.5h to 2h; the heating rate during the sintering process is 2°C / min to 5°C / min.
2. The processing method according to claim 1, It is characterized in that In step S1, the drying method is natural drying in the shade, and the drying time is 2 hours to 6 hours.
3. A treatment method according to claim 1 or 2, It is characterized in that The method comprises mixing the refractory aggregate, the binder, the suspending agent, the pore-forming agent, the thickener and the carrier liquid, and ball-milling the mixture to obtain the coating.
Citation Information
Patent Citations
Micro-jetting bonding forming method of ceramic mould core blank
CN105599106A
Manufacturing method and device for ceramic shell core for precision casting
CN111940683A
Water-based paint for 3D printing sand mold core and preparation process of water-based paint
CN114309454A