A non-fullerene acceptor material and its preparation method and application

By introducing ester groups and non-fullerene acceptor materials that extend the conjugation length into polymer solar cells, the problem of low open circuit voltage of the binary system is solved, the photoelectric conversion efficiency and open circuit voltage of organic solar cells are improved, and the Commercial application of high-efficiency, low-cost large-area solar cells.

CN116375732BActive Publication Date: 2024-10-11SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310282263.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-21
Publication Date
2024-10-11
Estimated Expiration
2043-03-21

AI Technical Summary

Technical Problem

The open circuit voltage of the binary system in existing polymer solar cells is low, which limits the improvement of the energy conversion efficiency of the device and makes it difficult to achieve large-scale commercial application.

Method used

A non-fullerene acceptor material is designed, which introduces ester groups and extends the conjugation length into the small molecule fused ring skeleton, using Stille coupling reaction, condensation ring closing reaction, reduction reaction, Vilsmeier-Haack reaction and Knoevenagel reaction, etc. Through step-by-step synthesis, an A-DA'D-A small molecule acceptor material with excellent film-forming properties and strong light absorption ability is obtained, which can be used to improve the open circuit voltage and photoelectric conversion efficiency of organic solar cells.

Benefits of technology

Achieved stronger absorption and higher photoelectric conversion efficiency in the ultraviolet-visible region (600-900nm), significantly improved the open circuit voltage and short circuit current of organic solar cells, and the device efficiency exceeded 15%, promoting large-area, low-cost , Development of high-efficiency solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GHA0000005305290000021
    Figure GHA0000005305290000021
  • Figure GHA0000005305290000022
    Figure GHA0000005305290000022
  • Figure GHA0000005305290000023
    Figure GHA0000005305290000023
Patent Text Reader

Abstract

The present invention belongs to the technical field of optoelectronic materials, and specifically relates to a non-fullerene acceptor material, a preparation method and an application thereof. The present invention introduces an ester group into a small molecule condensed ring skeleton and extends the conjugation length, and designs and synthesizes a series of A-DA'D-A type small molecule acceptor materials. The small molecule acceptor material in the present invention has good planarity, excellent film-forming properties, strong light absorption ability, stronger absorption in the ultraviolet-visible light region, and a more matching energy level with the existing common binary systems such as PM6:L8-BO, and can obtain a higher open circuit voltage and photoelectric conversion efficiency. It has good application prospects in the fields of preparing large-area organic solar cells, organic photodetectors, organic field-effect transistors and organic light-emitting diodes with high open circuit voltage and high energy conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of optoelectronic materials, and in particular to a non-fullerene acceptor material and a preparation method and application thereof. Background Art

[0002] In today's world, energy is an important factor in promoting economic development. As energy problems become increasingly serious, the development of new energy sources is urgent. Solar energy has many advantages, such as being clean, pollution-free, inexhaustible, and has great development prospects. Organic solar cells are a technical means of converting solar energy, a clean energy, into electrical energy. Organic solar cells have the advantages of being light, color-adjustable, flexible, low-cost, and highly efficient. Organic solar cells that can be prepared on a large scale have always been the goal pursued by people and have received widespread attention in the global academic and industrial circles.

[0003] Organic solar cells have broad application prospects in the future energy field. In recent years, due to the in-depth research on high-efficiency photovoltaic materials, device optimization and interface engineering, bulk heterojunction organic solar cells of polymer donors and non-fullerene small molecule acceptors have also developed rapidly. Although organic solar cells have great potential, there are still several key issues to be overcome to achieve their large-scale commercial application. Among the several factors that affect the photon-to-electron conversion efficiency (PCE) of polymer solar cells, the open circuit voltage (Voc) of the cell device has a particularly significant impact. Therefore, it is an important research direction to achieve a breakthrough in its efficiency by preparing organic solar cells with high Voc.

[0004] In the prior art, bulk heterojunction organic solar cells formed by combining polymer donors and small molecule acceptors have low open circuit voltages of binary system devices, which cannot further improve the energy conversion efficiency of the device. Therefore, developing a small molecule condensed ring skeleton with a good planar structure and further preparing a non-fullerene acceptor material with excellent solubility is of great significance for improving the Voc of organic solar cells to obtain higher PCE, preparing low-cost, large-area organic solar cells, and promoting their commercialization. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a non-fullerene acceptor material and a preparation method and application thereof. The present invention adopts a small molecule acceptor material with good planarity, excellent film-forming property and strong light absorption ability, which is characterized by introducing an ester group into the small molecule condensed ring skeleton and extending the conjugation length. The small molecule acceptor material in the present invention has stronger absorption in the ultraviolet-visible region (600-900nm) and has a higher photoelectric conversion efficiency, and has a more matching energy level and obtains a higher open circuit voltage with the existing common PM6:L8-BO and other binary systems. It has good application prospects in the fields of preparing large-area organic solar cells, organic photodetectors, organic field effect transistors and organic light-emitting diodes with high open circuit voltage and high energy conversion efficiency.

[0006] The first aspect of the present invention provides a non-fullerene acceptor material having a structure shown in formula (I):

[0007]

[0008] in,

[0009] R1, R2 are each independently selected from a linear or branched alkyl, alkoxy or thioalkyl group having 1 to 30 C atoms;

[0010] Ar1 and Ar2 are each independently selected from an aryl group, a heteroaryl group, or a condensed ring group having 5 to 30 ring atoms, wherein the aryl group, the heteroaryl group, or the condensed ring group is unsubstituted or optionally substituted with one or more S1;

[0011] The S1 is independently selected from H, F, Cl, Br, cyano, trifluoromethyl, or two of the S1 together form =O,

[0012] According to some embodiments of the present invention, R1 and R2 are each independently selected from a linear or branched alkyl group, an alkoxy group or a thioalkyl group having 5 to 20 C atoms.

[0013] Preferably, R1 is a straight-chain alkyl group having 10 to 15 C atoms;

[0014] The straight-chain alkyl group having 10 to 15 C atoms can be selected from the following groups:

[0015]

[0016] Preferably, R2 is a branched alkyl group having 5 to 10 C atoms;

[0017] The branched alkyl group having 5 to 10 C atoms may be selected from the following groups:

[0018]

[0019] The dotted line indicates the connection location.

[0020] More preferably, R1 is a straight chain alkyl group having 10 to 12 C atoms and R2 is a branched chain alkyl group having 7 to 9 C atoms.

[0021] According to some embodiments of the present invention, Ar1 and Ar2 are each independently selected from the following groups:

[0022]

[0023] in,

[0024] X1 and X2 are each independently selected from H, F, Cl, Br, cyano, and trifluoromethyl;

[0025] The dotted line indicates the connection location.

[0026] Preferably, Ar1 and Ar2 are

[0027] in,

[0028] X1 and X2 are each independently selected from F, Cl, Br, and trifluoromethyl.

[0029] The present invention adopts a small molecule receptor material with good planarity, excellent film-forming property and strong light absorption ability, and is characterized by introducing an ester group into the small molecule condensed ring skeleton and extending the conjugation length to design and synthesize a series of A-DA'DA type small molecule receptor materials. The non-fullerene receptor material of the present invention has stronger absorption in the ultraviolet-visible region (600-900nm) and has a higher photoelectric conversion efficiency.

[0030] The second aspect of the present invention provides a method for preparing the above-mentioned non-fullerene acceptor material, comprising the following steps:

[0031] S1, compound 1 and compound 2 undergo Stille coupling reaction in the presence of a catalyst to obtain compound 3;

[0032] S2, subjecting compound 3 to a condensation ring-closing reaction with triethyl phosphite, and then subjecting the compound 3 to a substitution reaction with a halogenated alkane X-R2 to obtain compound 4;

[0033] S3, reducing compound 4 with LiAlH4 to obtain intermediate 5;

[0034] S4, reacting the intermediate product 5 with diethyl 2,3-diisopropylsuccinate to obtain compound 6;

[0035] S5, compound 6 and a formylating agent are subjected to a Vilsmeier-Haack reaction to obtain compound 7;

[0036] S6, compound 7 and The acid-binding agent undergoes a Knoevenagel reaction to obtain a non-fullerene acceptor material represented by formula (I);

[0037]

[0038] R1, R2, X1, and X2 are as defined above.

[0039] According to some embodiments of the present invention, in step S1: the catalyst is selected from at least one of tetrakis(triphenylphosphine)palladium, palladium acetate, bis(triphenylphosphine)palladium dichloride, tris(dibenzylideneacetone)dipalladium, tri(o-tolyl)phosphine or cuprous iodide; preferably bis(triphenylphosphine)palladium dichloride.

[0040] According to some embodiments of the present invention, in step S1: the Stille coupling reaction is carried out in the presence of a solvent and under the protection of an inert gas or nitrogen; preferably, the solvent is selected from at least one of toluene, tetrahydrofuran, N,N-dimethylformamide, dichloromethane, 1,4-dioxane, and dimethyl sulfoxide.

[0041] According to some embodiments of the present invention, in step S1: the molar ratio of compound 2 to compound 1 is 1-4:1; the molar volume ratio of compound 1 to solvent is 1 mmol:10-30 mL; the ratio of the molar amount of the catalyst to the total molar amount of compound 1 and compound 2 is 1:60-80.

[0042] According to some embodiments of the present invention, in step S1: the reaction temperature of the Stille coupling reaction is 60-100° C., and the reaction time is 12-36 h.

[0043] According to some embodiments of the present invention, step S1 further comprises purification of compound 3, and the purification process comprises rotary evaporation, extraction and column chromatography separation.

[0044] According to some embodiments of the present invention, in step S2: the condensation ring-closing reaction is carried out in the presence of a solvent and under the protection of an inert gas or nitrogen. Preferably, the solvent is selected from at least one of o-dichlorobenzene, toluene and chlorobenzene.

[0045] According to some embodiments of the present invention, in step S2: the molar ratio of compound 3 to triethyl phosphite is 1:4-15, and the molar volume ratio of compound 3 to solvent is 1 mmol:10-20 mL.

[0046] According to some embodiments of the present invention, in step S2: the reaction temperature of the condensation ring-closing reaction is 160-200° C., and the reaction time is 6-18 hours.

[0047] According to some embodiments of the present invention, in step S2: the substitution reaction is carried out in the presence of a solvent and under the protection of an inert gas or nitrogen; preferably, the solvent is selected from at least one of N,N-dimethylformamide, dimethyl sulfoxide, and 1,4-dioxane.

[0048] According to some embodiments of the present invention, in step S2: wherein the molar ratio of the halogenated alkane R2X to the compound 3 is 10-20:1.

[0049] According to some embodiments of the present invention, in step S2: the reaction raw materials of the substitution reaction also include potassium iodide and potassium hydroxide; preferably, the molar ratio of potassium iodide to compound 3 is 1-2:1, and the molar ratio of potassium hydroxide to compound 3 is 30-40:1.

[0050] According to some embodiments of the present invention, in step S2: the reaction temperature of the substitution reaction is 60-120° C., and the reaction time is 6-18 h.

[0051] According to some embodiments of the present invention, step S2 further comprises purification of compound 4, and the purification process comprises extraction, rotary evaporation and column chromatography separation.

[0052] According to some embodiments of the present invention, in step S3: the reduction reaction is carried out in the presence of a solvent and under the protection of an inert gas or nitrogen; preferably, the solvent is selected from at least one of tetrahydrofuran and toluene.

[0053] According to some embodiments of the present invention, in step S3: the molar ratio of compound 4 to LiAlH4 is 1:15-25, and the molar volume ratio of compound 4 to solvent is 1 mmol:10-20 mL.

[0054] According to some embodiments of the present invention, in step S3: the reaction temperature of the reduction reaction is 60-90° C., and the reaction time is 6-18 hours.

[0055] According to some embodiments of the present invention, in step S4: the reaction is carried out in the presence of a solvent, preferably, the solvent is selected from at least one of ethanol, methanol and isopropanol.

[0056] According to some embodiments of the present invention, in step S4: the molar ratio of compound 4 to diisopropyl 2,3-dioxysuccinate is 1:2-4.

[0057] According to some embodiments of the present invention, in step S4: the reaction temperature of the reaction is 60-90° C., and the reaction time is 6-18 hours.

[0058] According to some embodiments of the present invention, step S4 further comprises purification of compound 6, and the purification process comprises extraction, rotary evaporation and column chromatography separation.

[0059] According to some embodiments of the present invention, in step S5: the formylating agent is phosphorus oxychloride.

[0060] According to some embodiments of the present invention, in step S5: the Vilsmeier-Haack reaction is carried out in the presence of a solvent; preferably, the solvent is selected from at least one of N,N-dimethylformamide, dimethyl sulfoxide, and 1,4-dioxane.

[0061] According to some embodiments of the present invention, in step S5: the mass ratio of compound 6 to the formylating agent is 1:2-6; the molar volume ratio of compound 6 to the solvent is 1 mmol:20-60 mL.

[0062] According to some embodiments of the present invention, in step S5: the Vilsmeier-Haack reaction is carried out at -4 to 10°C for 0.5 to 2 hours, and then at 60 to 120°C for 6 to 18 hours.

[0063] According to some embodiments of the present invention, step S5 further comprises purification of compound 7, and the purification process comprises extraction, rotary evaporation and column chromatography separation.

[0064] According to some embodiments of the present invention, in step S6: the acid binding agent is selected from at least one of pyridine and piperidine.

[0065] According to some embodiments of the present invention, in step S6: the Knoevenagel reaction is carried out in the presence of a solvent and under the protection of an inert gas or nitrogen; preferably, the solvent is selected from at least one of chloroform, toluene and dichloromethane.

[0066] According to some embodiments of the present invention, in step S6: the molar amount of compound 7 and The molar ratio of compound 7 to solvent is 1:3-6, the molar volume ratio of compound 7 to solvent is 1 mmol:150-300 mL, and the molar volume ratio of compound 7 to acid binding agent is 1 mmol:5-15 mL.

[0067] According to some embodiments of the present invention, in step S6: the reaction temperature of the Knoevenagel reaction is 50-90° C., and the reaction time is 6-18 hours.

[0068] According to some embodiments of the present invention, step S6 further includes purification of the non-fullerene acceptor material represented by formula (I), and the purification process includes crystallization using methanol and column chromatography separation.

[0069] The non-fullerene acceptor material of the present invention has mild reaction conditions for synthesis, simple operation, easy implementation of scale-up production, and high yield.

[0070] The third aspect of the present invention provides the use of the above-mentioned non-fullerene acceptor material in the preparation of organic / polymer solar cells, perovskite solar cells, organic photodetectors, organic field effect transistors and organic light emitting diodes.

[0071] The non-fullerene acceptor material of the present invention is used as the third component in a ternary organic solar cell system to increase the open circuit voltage of the device, and is also used in large-area solar cell devices.

[0072] A fourth aspect of the present invention provides an organic solar cell, comprising an active layer, wherein the active layer comprises the non-fullerene acceptor material described above.

[0073] Furthermore, the organic solar cell comprises, from bottom to top, a transparent substrate, a hole transport layer, the active layer, an electron transport layer and a metal electrode.

[0074] According to some embodiments of the present invention, the active layer further comprises an organic solar cell binary system;

[0075] Preferably, the polymer donor of the organic solar cell binary system is selected from at least one of PM6, PBTB-T-2F, PBDB-T, D18, and PTQ-10, and the acceptor is selected from at least one of Y6, L8-BO, and BTP-eC9.

[0076] The non-fullerene acceptor material of the present invention has a more matching energy level and obtains a higher open circuit voltage with the existing common PM6:L8-BO binary system, and has a good application prospect in the field of preparing large-area organic solar cells with high open circuit voltage and high energy conversion efficiency.

[0077] Beneficial effects:

[0078] (1) The non-fullerene acceptor material of the present invention is soluble in common solvents such as chloroform and chlorobenzene and is easy to process;

[0079] (2) The non-fullerene acceptor material of the present invention adopts a small molecule structure with good planarity, good film-forming property and low exciton binding energy. The material is characterized by a small molecule acceptor with an isopropoxycarbonyl group attached to a quinoxaline ring. Due to the strong electronegativity of the isopropoxycarbonyl group (stronger than that of the imide structure), the non-fullerene acceptor material of the present invention has a deeper HOMO energy level. Therefore, it can be used as the third component in a ternary solar cell system to increase the open circuit voltage of the device. At the same time, the non-fullerene acceptor material of the present invention has a wide absorption spectrum range, and the device can obtain a higher short-circuit current.

[0080] (3) The non-fullerene acceptor material of the present invention, when added to the existing binary system, greatly improves the charge separation and transfer efficiency of the device, significantly increases the open circuit voltage, and realizes an organic solar cell with an efficiency exceeding 15%, which is of great significance for the preparation of low-cost, large-area, high-efficiency battery devices;

[0081] (4) The present invention obtains a ternary material system for an organic solar cell with a high open circuit voltage to develop a high-efficiency, large-area organic solar cell to promote the device to obtain a higher device efficiency.

[0082] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0083] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0084] Figure 1 Compound 6 prepared in Example 1 of the present invention 1 H-NMR characterization spectrum;

[0085] Figure 2 The non-fullerene acceptor material DOXCT-4F prepared in Example 1 H-NMR characterization spectrum;

[0086] Figure 3 The non-fullerene acceptor material DOXCT-4Cl prepared in Example 1 H-NMR characterization spectrum;

[0087] Figure 4 The UV-visible absorption spectrum of the non-fullerene acceptor material film prepared in Example;

[0088] Figure 5 It is a schematic diagram of the structure of an organic solar cell device of the present invention;

[0089] Figure 6The JV curve of the non-fullerene acceptor material prepared in the example and applied to organic solar cells. DETAILED DESCRIPTION

[0090] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0091] The synthesis method of the non-fullerene acceptor material is as follows:

[0092]

[0093] Example 1

[0094] The preparation of the non-fullerene organic small molecule receptor material DOXCT-4F, the reaction process is as follows:

[0095]

[0096] Synthesis of compound 3: In a 250mL round-bottom flask, weigh compound 1 (2g, 5.2mmol) and compound 2 (7.59g, 13.02mmol) and dissolve in 100mL toluene, replace the gas, pass argon for 15 minutes, and add bistriphenylphosphine palladium dichloride (0.3g, 0.25mmol) to the reaction system under argon protection. The reactants were refluxed at 80°C for 24 hours. Cool to room temperature, spin dry tetrahydrofuran, extract with dichloromethane, spin dry the solvent to obtain a crude product, separate and purify by silica gel column chromatography to obtain a solid product, namely compound 3 (2.92g, 78%); HRMS (m / z, MALDI): Calc.for C 40 H 52 N2S5, [M+H] + :721.17, found:720.27.

[0097] Synthesis of compound 4: Compound 3 (2 g, 2.8 mmol) was dissolved in a three-necked flask containing o-dichlorobenzene (o-DCB, 50 mL) under Ar protection, and the temperature was raised to 180°C. Triethyl phosphite (4.2 g, 25.0 mmol) was slowly dripped into the reaction system, refluxed and stirred for 12 h, cooled to room temperature, and distilled under reduced pressure at 100°C (no need to pass through a column, directly proceed to the next step) to obtain an intermediate product. The intermediate product, 1-bromo-2-ethylhexane (7.5 g, 38.5 mmol), potassium iodide (0.56 g, 3.4 mmol) were added to the reaction mixture. l) and potassium hydroxide (4.8 g, 91.6 mmol) were dissolved in a single-necked flask containing N,N-dimethylformamide (DMF, 90 mL), and refluxed at 90°C under Ar protection overnight. The reactant was then cooled to room temperature and extracted with dichloromethane and water. Finally, the organic layers were combined and the solvent was dried by spin drying. The crude product was purified by silica gel column using DCM / PE (1 / 5, v / v) as eluent. After the eluent was dried by spin drying, a light yellow solid compound 4 (1.07 g, 41%) was obtained; HRMS (m / z, MALDI): Calc. for C 56 H 82 N4S5,[M+H] + :971.60, found:970.50.

[0098] Synthesis of compound 6: Under nitrogen conditions, compound 4 (2.0 g, 2.06 mmol), LiAlH4 (1.56 g, 41.17 mmol) and 30 mL of THF were added to a 100 mL flask. The mixed solution was stirred at 75 ° C for 12 h, cooled to room temperature, extracted with dichloromethane, dried with anhydrous Na2SO4, filtered and concentrated under reduced pressure. Intermediate 5 was obtained and used directly to synthesize compound 6. Subsequently, compound 5 was subjected to condensation coupling reaction with diisopropyl 2,3-dioxysuccinate (1.46 g, 6.36 mmol) in ethanol (30 mL) at 80 ° C. After 12 h, the organic phase was separated by extraction with dichloromethane and then dried over Na2SO4. Finally, dichloromethane was removed under reduced pressure to obtain a red solid, which was further purified by column chromatography (petroleum ether / dichloromethane, v / v=2:1). (1.62 g, 70%). H NMR spectrum is as follows Figure 1 As shown, MALDI-TOF-MS: m / z=1136.730 (M + ).

[0099] Synthesis of compound 7: In a 100 mL three-necked flask, add compound 6 (0.50 g, 0.44 mmol) and anhydrous N,N-dimethylformamide (25 mL), stir at 0°C for a few minutes, then add phosphorus oxychloride (1.5 mL). After stirring the reaction solution at 0°C for 1 hour, raise the temperature to 90°C and stir overnight, cool to room temperature, extract with dichloromethane, spin dry the solvent, separate and purify by silica gel column chromatography to obtain compound 7 (0.45 g, 86%), HRMS (m / z, MALDI): Calc.for: C 68 H 96 N4O6S4,[M+H] + :1193.78,found:1193.62.

[0100] Synthesis of receptor material DOXCT-4F: In a 100 mL round-bottom flask, compound 7 (300 mg, 0.25 mmol) and 5,6-difluoro-3-(dicyanomethylidene)indone (389.2 mg, 1.01 mmol) were dissolved in 50 mL of chloroform, the gas was replaced three times, argon protection was used, and 2.5 mL of pyridine was slowly added while stirring. The mixture was refluxed under argon protection for 12 h, cooled to room temperature, poured into 300 mL of anhydrous methanol, and filtered to obtain a crude product, which was separated and purified by silica gel column chromatography to obtain a dark blue solid, which was the receptor material DOXCT-4F (304.7 mg, 75%); H NMR spectrum was as follows Figure 2 As shown, HRMS (m / z, MALDI): Calc.for: C 92 H 100 F4N8O6S4,[M+H] + :1618.10,found:1616.66.

[0101] Example 2

[0102] The preparation of the non-fullerene organic small molecule receptor DOXCT-4Cl, the reaction process is as follows:

[0103]

[0104] Synthesis of compound 3: In a 250 mL round-bottom flask, weigh compound 1 (2 g, 5.2 mmol) and compound 2 (7.59 g, 13.02 mmol) and dissolve in 100 mL tetrahydrofuran, replace the gas, pass argon for 15 minutes, and add bistriphenylphosphine palladium dichloride (0.3 g, 0.25 mmol) to the reaction system under argon protection. The reactants were refluxed at 80 ° C for 24 hours. Cool to room temperature, spin dry tetrahydrofuran, extract with dichloromethane, spin dry the solvent to obtain a crude product, separate and purify by silica gel column chromatography to obtain a solid product, namely compound 3 (2.92 g, 78%); HRMS (m / z, MALDI): Calc.for C 40 H 52 N2S5, [M+H] + :721.17, found:720.27.

[0105] Synthesis of compound 4: Compound 3 (2 g, 2.8 mmol) was dissolved in a three-necked flask containing o-dichlorobenzene (o-DCB, 50 mL) under Ar protection, and the temperature was raised to 180°C. Triethyl phosphite (4.2 g, 25.0 mmol) was slowly dripped into the reaction system, refluxed and stirred for 12 h, cooled to room temperature, and distilled under reduced pressure at 100°C (no need to pass through a column, directly proceed to the next step) to obtain an intermediate product. The intermediate product, 1-bromo-2-ethylhexane (7.5 g, 38.5 mmol), potassium iodide (0.56 g, 3.4 mmol) were added to the reaction mixture. l) and potassium hydroxide (4.8 g, 91.6 mmol) were dissolved in a single-necked flask containing N,N-dimethylformamide (DMF, 90 mL), and refluxed at 90°C under Ar protection overnight. The reactant was then cooled to room temperature and extracted with dichloromethane and water. Finally, the organic layers were combined and the solvent was dried by spin drying. The crude product was purified by silica gel column using DCM / PE (1 / 5, v / v) as eluent. After the eluent was dried by spin drying, a light yellow solid compound 4 (1.07 g, 41%) was obtained; HRMS (m / z, MALDI): Calc. for C 56 H 82 N4S5,[M+H] + :971.60, found:970.50.

[0106] Synthesis of compound 6: Under nitrogen conditions, compound 4 (2.0 g, 2.06 mmol), LiAlH4 (1.56 g, 41.17 mmol) and 30 mL THF were added to a 100 mL flask. The mixed solution was stirred at 75 ° C for 12 h, cooled to room temperature, extracted with dichloromethane, dried with anhydrous Na2SO4, filtered and concentrated under reduced pressure. Intermediate 5 was obtained and directly used to synthesize compound 6. Subsequently, compound 5 was subjected to condensation coupling reaction with diisopropyl 2,3-dioxysuccinate (1.46 g, 6.36 mmol) in ethanol (30 mL) at 80 ° C. After 12 h, the organic phase was separated by extraction with dichloromethane and then dried over Na2SO4. Finally, dichloromethane was removed under reduced pressure to obtain a red solid, which was further purified by column chromatography (petroleum ether / dichloromethane, v / v=2:1). (1.62 g, 70%).

[0107] 1 H NMR (400MHz, CDCl3), δ (ppm): 7.03 (s, 2H), 5.50–5.44 (m, 2H), 4.70–4.61 (m, 4H), 2.87–2.83 (t, 4H), 2.09–2. 06(t,2H),1.89–1.85(t,4H),1.55–1.54(d,6H),1.38–1.11(m,36H),1.10–0.86(m,24H),0.64–0.60(m,12H).

[0108] 13 C NMR (100MHz, CDCl3), δ (ppm): 165.32, 143.79, 140.86, 137.88, 136.97, 134.77, 131.73, 123.26, 122.44, 119.44, 117.37, 69.93, 55.00, 3 9.91,31.92,29.70,29.67,29.64,29.63,29.51,29.50,29.37,28.84 ,27.73,27.70,23.05,22.99,22.75,22.70,21.86,14.12,13.76,S-4 10.05,10.00.

[0109] MALDI-TOF-MS: m / z = 1136.730 (M + ).

[0110] Synthesis of compound 7: In a 100mL three-necked flask, add compound 6 (0.50g, 0.44mmol) and anhydrous N,N-formamide (25mL), stir at 0℃ for a few minutes, then add phosphorus oxychloride (1.5mL). After stirring the reaction solution at 0℃ for 1 hour, the temperature was raised to 90℃ and stirred overnight, cooled to room temperature, extracted with dichloromethane, the solvent was dried, and separated and purified by silica gel column chromatography to obtain compound 7 (0.45g, 86%); HRMS (m / z, MALDI): Calc.for: C 68 H 96 N4O6S4,[M+H] + :1193.78,found:1193.62.

[0111] Synthesis of acceptor material DOXCT-4Cl: In a 100 mL round-bottom flask, compound 7 (300 mg, 0.25 mmol) and 5,6-difluoro-3-(dicyanomethylidene)indone (389.2 mg, 1.01 mmol) were dissolved in 50 mL of chloroform, the gas was replaced three times, argon protection was used, and 2.5 mL of pyridine was slowly added while stirring. The mixture was refluxed under argon protection for 12 h, cooled to room temperature, poured into 300 mL of anhydrous methanol, and filtered to obtain a crude product, which was separated and purified by silica gel column chromatography to obtain a dark blue solid, which was the acceptor material DOXCT-4Cl (296.2 mg, 70%). The hydrogen nuclear magnetic resonance spectrum was as follows: Figure 3 As shown; HRMS (m / z, MALDI): Calc.for: C 92 H 100 C l4 N8O6S4, [M+H]+: 1683.90, found: 1682.54.

[0112] Test Example 1

[0113] UV-vis absorption spectroscopy analysis was performed on the receptor materials DOXCT-4F and DOXCT-4Cl in Examples 1 and 2. Receptor material film preparation: The chloroform solution (20 mg / mL) of the receptor material was spin-coated on quartz glass. The prepared receptor film was used for testing. The results are shown in FIG. Figure 4 As shown: it has stronger absorption in the UV-visible region (600-900nm). At the same time, the absorption curve of the small molecule DOXCT-4F in the film state is significantly red-shifted compared with DOXCT-4Cl, which indicates that the interaction between the molecular backbone and the π-π bond in the film state causes stronger stacking, which increases the interaction between electrons within the molecule. This indicates that DOXCT-4F has a stronger ability to accept electrons, and the asymmetric structure makes the molecule polar and thus produces a dipole moment, which is beneficial to charge transfer and thus improves Jsc.

[0114] The electrochemical performance of the receptor materials DOXCT-4F and DOXCT-4Cl was tested by cyclic voltammetry (CV). First, 0.1M tetrabutylammonium hexafluorophosphate (Bu4NPF6) was dissolved in 25mL of anhydrous acetonitrile (CH3CN) solution, Ag / AgCl was used as the reference electrode, and the platinum electrode was used as the counter electrode. The compound was dissolved in chloroform solution and then evenly applied on the glassy carbon electrode. The glassy carbon electrode was used as the working electrode. Ferrocene / ferrocene (Fc / Fc + ) was used as the redox internal standard. The oxidation potential E of DOXCT-4F was measured onset ox is 1.23 V, and the oxidation potential E of DOXCT-4Cl onset ox is 1.26V. According to the equation: E HOMO =-(4.80-E1 / 2, Fc / Fc + +E onset ox )(eV), the HOMO energy level of DOXCT-4F is calculated to be -5.67eV, and the HOMO energy level of DOXCT-4Cl is -5.64eV. They have good energy level matching with the donor material, and the lower HOMO energy enables the device to obtain a higher Voc.

[0115] Test Example 2

[0116] The non-fullerene acceptor material prepared by the present invention can be used to prepare an organic solar cell, which comprises, from bottom to top, a transparent substrate, a hole transport layer, an active layer, an electron transport layer and a metal electrode, such as Figure 5 as shown in .

[0117] The preparation and characterization of small-area OPV devices are as follows:

[0118] The commercially purchased indium tin oxide (ITO) glass was first scrubbed with acetone, and then ultrasonically cleaned with detergent, water, deionized water, acetone, and isopropanol in sequence. After drying, a 30nm thick PEDOT:PSS layer was spin-coated as an anode modification layer for standby use. A chloroform mixed solution (10-30mg / mL) of polymer donor materials PM6, L8-BO, the acceptor material prepared in the embodiment (weight ratio of 1:0.9:0.3) and additive chloronaphthalene (0.25%-3%) was spin-coated on the PEDOT:PSS anode modification layer to form the active layer of the device. Finally, a layer of PNDIT-F3N with a thickness of about 10nm was spin-coated as a cathode modification layer and Ag (100nm) as a device cathode to obtain a solar cell device cell structure: ITO / PEDOT:PSS / active layer / PNDIT-F3N / Ag).

[0119] The structures of the polymer donor material PM6 and the acceptor L8-BO electron transport layer PNDIT-F3N used in the above organic solar cell device are as follows:

[0120]

[0121] The energy conversion efficiency of solar cells is calculated using Guangyan SS-F5-3A as a solar simulator at 100mW / cm 2 The photovoltaic performance of the device was tested under light intensity, and the light intensity was calibrated by a standard single-crystal silicon solar cell (SRC-00019); the JV curve was measured using Keithley 2400. The open circuit voltage, short circuit current and fill factor of the above solar cell device were obtained from the test, and the corresponding photoelectric conversion efficiency was calculated.

[0122] The JV curve of a solar cell device is as follows: Figure 6 As shown in Table 1, it can be seen that the open circuit voltage V OC =0.85V, short circuit current J SC =23.53mA / cm 2 , fill factor FF = 78%, conversion efficiency PCE = 15.83%. The open circuit voltage V of the solar cell device with DOXCT-4F as the third component of the PM6:L8-BO active layer OC =0.90V, short circuit current J SC =23.93mA / cm 2 , fill factor FF = 75%, conversion efficiency PCE = 16.35%. The open circuit voltage V of the solar cell device with DOXCT-4Cl as the third component of the PM6:L8-BO active layer OC =0.90V, short circuit current J SC =23.63 mA / cm2, filling factor FF=75%, conversion efficiency PCE=16.19%. It can be seen that the acceptor material in the present invention as the third component can obtain a higher Voc than the binary system.

[0123] Table 1

[0124] Devices <![CDATA[J SC (mA cm -2 )]]> <![CDATA[V OC (V)]]> FF PCE(%) PM6:L8-BO 23.53 0.85 0.78 15.83 PM6:L8-BO:DOXCT-4F 23.93 0.90 0.75 16.35 PM6:L8-BO:DOXCT-4Cl 23.63 0.90 0.75 16.19

[0125] Test Example 3

[0126] The preparation and characterization of large-area printed OPV devices are as follows:

[0127] 20cm 2The IT0 conductive glass was ultrasonically cleaned with acetone, ethanol, and deionized water for 10 to 20 minutes, dried with nitrogen, and then treated with ultraviolet ozone for 10 minutes; a 30nm thick PEDOT:PSS layer was spin-coated on the substrate as a hole transport layer for standby use. The polymer donor material PM6, L8-BO and the acceptor material prepared in the embodiment (weight ratio of 1:0.9:0.3) and the additive chloronaphthalene (0.25%-3%) in chloroform (10-30mg / mL) were printed on the PEDOT:PSS layer to form an active layer of 300nm thick. PNDIT-F3N was dissolved in methanol solution and 0.5% acetic acid was added to prepare a 1moL / mL solution, and the solution was spin-coated on the surface of the active layer at a speed of 4000 revolutions per second, and then annealed at 100°C for 10min to prepare an electron transport layer with a thickness of 8nm. Finally, the Ag electrode was prepared by printing technology, using silver paste as the raw material. A layer of silver paste is directly brushed on the surface of the prepared electron transport layer as an electrode, and the thickness of the electrode layer is 100 nm.

[0128] Performance test of large-area devices: select a large-area battery for testing under standard test conditions: AM1.5, 100mW / cm 2 , the open circuit voltage of the device is measured (V OC )=0.76V, short circuit current (J SC )=17.80mA / cm 2 , fill factor (FF) = 0.74, photoelectric conversion efficiency (PCE) = 10.02%.

[0129] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A non-fullerene acceptor material, characterized in that: It has the structure shown in formula (I): Formula (I); in, R1 is a straight-chain alkyl group having 10 to 15 C atoms, and R2 is a branched alkyl group having 5 to 10 C atoms; Ar1 and Ar2 are , in, X1 and X2 are each independently selected from F, Cl, Br, and trifluoromethyl.

2. The method for preparing a non-fullerene acceptor material according to claim 1, characterized in that: The following steps are involved: S1, compound 1 and compound 2 are reacted in the presence of a catalyst to obtain compound 3; S2, subjecting compound 3 to a condensation ring-closing reaction with triethyl phosphite, and then subjecting the compound 3 to a substitution reaction with a halogenated alkane X-R2 to obtain compound 4; S3, reducing compound 4 with LiAlH4 to obtain intermediate product 5; S4, intermediate product 5 and Reaction to obtain compound 6; S5, compound 6 and a formylating agent are subjected to a Vilsmeier-Haack reaction to obtain compound 7; S6, compound 7 and , and an acid-binding agent to carry out a Knoevenagel reaction to obtain a non-fullerene acceptor material represented by formula (I); ; R1, R2, X1, and X2 are as defined in claim 1.

3. The preparation method according to claim 2, characterized in that: In step S1, the catalyst is selected from at least one of tetrakis(triphenylphosphine)palladium, palladium acetate, bis(triphenylphosphine)palladium dichloride, tris(dibenzylideneacetone)dipalladium, tri(o-tolyl)phosphine or cuprous iodide; And / or, in step S5, the formylation agent is phosphorus oxychloride; And / or, in step S6, the acid binding agent is selected from at least one of pyridine and piperidine.

4. Use of the non-fullerene acceptor material according to claim 1 in the preparation of organic / polymer solar cells, perovskite solar cells, organic photodetectors, organic field effect transistors and organic light emitting diodes.

5. An organic solar cell comprising an active layer, characterized in that: The active layer comprises the non-fullerene acceptor material according to claim 1.

6. The organic solar cell according to claim 5, characterized in that The active layer also includes an organic solar cell binary system.

7. The organic solar cell according to claim 6, characterized in that The polymer donor of the organic solar cell binary system is selected from at least one of PM6, PBTB-T-2F, PBDB-T, D18, and PTQ-10, and the acceptor is selected from at least one of Y6, L8-BO, and BTP-eC9.