An organic receptor material and its preparation method and application
By developing fused ring non-fullerene acceptor materials, the problems of component interaction and solvent compatibility in ternary organic solar cells have been solved, the charge separation and transmission efficiency has been improved, and high-efficiency organic solar cells have been achieved, which are suitable for large-scale applications. Commercial applications of area batteries.
Patent Information
- Application Number
- CN202310285499.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-15
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-15
AI Technical Summary
In the research of ternary organic solar cells, there are challenges such as component interaction, compatibility of active layer materials and solvents, and the impact of the third component on charge dynamics, which affect device performance and commercial development.
Develop a fused ring non-fullerene acceptor material, which is prepared through steps such as Knoevenagel reaction, Vilsmeier-Haack reaction and Stille coupling reaction to produce small organic molecules with planarity, good film-forming properties and low exciton binding energy. Acceptor materials are used to increase device efficiency and are combined with polymer donors and other layers to form high-efficiency solar cell active layers.
It achieves a high efficiency of organic solar cells exceeding 17%, avoids the problems of moisture absorption, acid-base and environmental instability of the interface layer, and is suitable for the preparation of large-area, high-efficiency battery devices.
Smart Images

Figure CN116375741B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cells, and in particular to an organic receptor material and a preparation method and application thereof. Background Art
[0002] With the over-exploitation of fossil energy, the development of environmentally friendly renewable energy is urgent. Organic solar cells (OSCs) have attracted more and more attention from researchers due to their advantages such as light weight, low price, wide source, flexibility and simple preparation process. As a new third-generation photovoltaic technology, it has broad application prospects in the future energy field. In recent years, in addition to the development of new high-efficiency photovoltaic donor / acceptor materials, the process of preparing ternary devices by adding a third component material is considered to be an effective method to improve the photoelectric conversion efficiency. Researchers blend materials with complementary energy levels and complementary absorption in the same active layer, which is beneficial to improve the photoelectric conversion efficiency (PCE) of the device.
[0003] Ternary organic solar cells (TOSCs) not only retain the simple and easy preparation method of traditional binary devices, but also have the characteristics of expanding the light absorption range, adjusting the energy level matching of the D / A interface, and optimizing the morphology. They are an important way to achieve high power conversion efficiency. However, there are still many problems in the research of ternary organic solar cells: (1) The interaction between the components of the ternary device has a great influence on the performance of the device, and the rational screening of the third component to regulate the morphology of the active layer still requires in-depth research; (2) The compatibility of the active layer materials of the ternary device with solvents is particularly important. The selection of solvents that can be commercialized and can improve device performance is the key to the development of organic solar cells; (3) Understanding the impact of the third component on the charge dynamics of the main system is also important for the ternary strategy to improve device performance.
[0004] Therefore, it is necessary to develop a condensed-ring non-fullerene acceptor material as the third component to improve the efficiency of organic solar cell devices. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the first aspect of the present invention provides an organic acceptor material, which promotes the device to obtain a higher device efficiency and is applied to large-area organic solar cells.
[0006] The second aspect of the present invention also provides a method for preparing an organic receptor material.
[0007] The third aspect of the present invention also provides an application of an organic acceptor material in a solar cell.
[0008] A fourth aspect of the present invention also provides a solar cell active layer.
[0009] A fifth aspect of the present invention also provides a solar cell.
[0010] The organic receptor material provided in the embodiment according to the first aspect of the present invention includes a compound as shown in formula (I);
[0011]
[0012] Wherein R1 and R3 are independently selected from substituted or unsubstituted C 1~30 Alkyl, substituted or unsubstituted C 1~30 Alkoxy, substituted or unsubstituted C 2~10 Alkenyl, substituted or unsubstituted C 2~30 Alkynyl, substituted or unsubstituted C 6~30 The aromatic group;
[0013] R2 is selected from substituted or unsubstituted C 6~30 Aryl, substituted or unsubstituted C 6~30 heteroaryl;
[0014] A1 and A2 are independently selected from substituted or unsubstituted C 6~30 Aryl, substituted or unsubstituted C 6~30 The heteroaryl group.
[0015] The organic receptor material according to the embodiment of the present invention has at least the following beneficial effects:
[0016] The organic acceptor material provided by the present invention is soluble in common solvents such as chloroform and chlorobenzene, and is easy to process; it has good thermal stability; it adopts a small molecule structure with good planarity, good film-forming property and low exciton binding energy; in addition, the organic acceptor material greatly improves the charge separation and transmission efficiency of the device, and avoids the shortcomings of the interface layer of the existing high-efficiency device such as hygroscopicity, acidity and alkalinity, batch repeatability, environmental instability, etc., and realizes an organic solar cell with an efficiency of more than 17%, which is of great significance for the preparation of large-area, high-efficiency battery devices.
[0017] According to some embodiments of the present invention, R1 and R3 are independently selected from substituted or unsubstituted C 1~10 Alkyl, substituted or unsubstituted C 1~10 Alkoxy, substituted or unsubstituted C 2~5 Alkenyl, substituted or unsubstituted C 2~10 Alkynyl, substituted or unsubstituted C 6~10 The aromatic group;
[0018] According to some embodiments of the present invention, A1 and A2 are selected from one of the following structural formulas:
[0019]
[0020] Wherein, X1 and X2 are independently selected from H, halogen, cyano, substituted or unsubstituted C 1~30 Alkyl, substituted or unsubstituted C 1~30 of alkoxy.
[0021] According to some embodiments of the present invention, R2 is selected from substituted or unsubstituted C 6~10 Aryl, substituted or unsubstituted C 6~10 heteroaryl;
[0022] According to some embodiments of the present invention, R2 is selected from one of the following structural formulas:
[0023]
[0024] Wherein R4 is selected from substituted or unsubstituted C 1~30 Alkyl, substituted or unsubstituted C 1~30 of alkoxy.
[0025] According to some embodiments of the present invention, the compound I is selected from one of the following structural formulas:
[0026]
[0027] According to the second aspect of the present invention, the method for preparing an organic receptor material provided by the embodiment comprises the following steps:
[0028] S6, adding compound 7, compound A1 or A2, a first organic solvent and pyridine, and obtaining an organic acceptor material by Knoevenagel reaction under an inert gas;
[0029]
[0030] According to some embodiments of the present invention, the first organic solvent is selected from at least one of chloroform, toluene and chlorobenzene.
[0031] According to some embodiments of the present invention, the compound 7 is prepared by the following method:
[0032] S5, adding compound 6, adding DMF, and then adding a second organic solvent; adding POCl3 dropwise under the protection of an inert gas, performing a Vilsmeier-Haack reaction, drying after the reaction, extracting, and purifying by a chromatographic column to obtain compound 7;
[0033] The structural formula of compound 6 is as follows:
[0034]
[0035] According to some embodiments of the present invention, the second organic solvent includes 1,2-dichloroethane.
[0036] According to some embodiments of the present invention, the compound 6 is prepared by the following method:
[0037] S4, adding compound 5, triethyl phosphite, Br-R3, and then adding a third organic solvent, and reacting under reflux under inert gas protection. After the reaction is completed, drying, extraction, and chromatography column purification are performed to obtain compound 6;
[0038] The structural formula of compound 5 is as follows:
[0039]
[0040] According to some embodiments of the present invention, the above-mentioned tert-butyl compound is prepared by an organic solvent such as chlorobenzene.
[0041] S3, adding compound 3, compound 4, a catalyst and a ligand, and then adding a fourth organic solvent, reacting under inert gas protection, undergoing Stille coupling reaction, drying after the reaction is completed, extracting, and purifying by chromatographic column to obtain compound 5;
[0042] Among them, the structural formulas of compound 3 and compound 4 are as follows:
[0043]
[0044] According to some embodiments of the present invention, the catalyst is selected from at least one of tetrakis(triphenylphosphine)palladium, palladium acetate, bis(triphenylphosphine)palladium dichloride, tris(dibenzylideneacetone)dipalladium and tri(o-tolyl)phosphine or cuprous iodide.
[0045] According to some embodiments of the present invention, the compound 3 is prepared by the following method:
[0046] S2, adding compound 2, concentrated sulfuric acid and concentrated nitric acid, reacting for a period of time, then adding concentrated sulfuric acid and potassium nitrate, reflux reaction, drying after the reaction, extracting, and purifying by chromatographic column to obtain compound 3;
[0047] According to some embodiments of the present invention, the structural formula of compound 2 is as follows:
[0048]
[0049] According to some embodiments of the present invention, the compound 2 is prepared by the following method:
[0050] S1, adding 2-amino-3,6-dibromobenzenethiol, alkyl aldehyde R1-CHO and hexadecyltrimethylammonium bromide to react in an aqueous solution, drying after the reaction, extracting, and purifying by a chromatographic column to obtain compound 2;
[0051] According to some embodiments of the present invention, the structural formula of compound 1 is as follows:
[0052]
[0053] The third aspect of the present invention provides the use of the above-mentioned organic acceptor material in a solar cell.
[0054] A fourth aspect of the present invention provides a solar cell active layer, comprising an acceptor material and a polymer donor, wherein the acceptor material is selected from any one of the organic acceptor materials described above.
[0055] According to some embodiments of the present invention, the polymer donor is selected from at least one of PM6, PBDB-T, D18, and PTQ-10.
[0056] The structural formulas of PM6, PBDB-T, D18 and PTQ-10 are as follows:
[0057]
[0058] A fifth aspect of the present invention provides an organic solar cell, which comprises a substrate, a hole transport layer, an active layer, an electron transport layer and a metal electrode in sequence; the active layer is selected from the solar cell active layer described above.
[0059] According to some embodiments of the present invention, the substrate is at least one of indium tin oxide (ITO) glass and fluorine tin oxide (FTO).
[0060] According to some embodiments of the present invention, the hole transport layer is selected from at least one of PEDOT:PSS, MoO3, V2O5, WO3 and NiO.
[0061] According to some embodiments of the present invention, the electron transport layer is selected from at least one of PFN-Br, PNDIT-F3N or PDINO.
[0062] Among them, the structural formula of PFN-Br, PNDIT-F3N or PDINO is as follows:
[0063]
[0064] According to some embodiments of the present invention, the metal electrode is selected from at least one of Ag, Al or Cu.
[0065] Definitions and general terms
[0066] As used herein, "substituted or unsubstituted" means that a group may or may not be further substituted by one or more groups selected from the group consisting of alkyl, alkenyl, alkynyl, aryl, halogen, haloalkyl, haloalkenyl, haloalkynyl, haloaryl, hydroxy, alkoxy, alkenyloxy, aryloxy, benzyloxy, haloalkoxy, haloalkenyloxy, haloaryloxy, nitro, nitroalkyl, nitroalkenyl, nitroalkynyl, nitroaryl, nitroheterocyclyl, amino, alkylamino, dialkylamino, alkenylamino, alkynylamino, arylamino, diarylamino, phenylamino, diphenylamino, benzylamino, dibenzylamino, hydrazino, acyl, acylamino, diacylamino, acyloxy, heterocyclyl, heterocyclyloxy, heterocyclylamino, haloheterocyclyl, carboxyl ester, carboxyl, carboxylamide, thiol, alkylthio, benzylthio, acylthio, and phosphorus-containing groups.
[0067] "Substituted or unsubstituted C 1~30 "alkyl" means an alkyl group having 1 to 30 carbon atoms, including C 1~30 Straight chain alkyl, C 1~30 The branched alkyl and C 3~30 wherein at least one H in the optional alkyl group is substituted by a group as defined herein, and for “substituted or unsubstituted C 1~10 The "alkyl group" has a similar explanation, except that the number of carbon atoms is different.
[0068] "Substituted or unsubstituted C 1~30 "Alkoxy" means an alkoxy group having a total carbon atom count of 1 to 30, including C1 to 30 straight chain alkoxy, C 1~30 Branched alkoxy and C 2~30 The cycloalkoxy group may be, for example, methoxy, ethoxy, n-propoxy, isopropoxy, etc. And at least one H in the optional alkoxy group is substituted by a group defined herein. 1~10 The "alkoxy group" has a similar explanation, except that the number of carbon atoms is different.
[0069] The "halogen" includes any one or two or more of fluorine, chlorine, bromine and iodine.
[0070] "Substituted or unsubstituted C 2~10 The term "alkenyl" refers to a straight or branched hydrocarbon group having one or more double bonds, wherein the total number of carbon atoms in the group is 2 to 10, the double bonds in the group may be in any position, and the optional C 2~10 At least one H in the alkenyl group is substituted by a corresponding group as defined herein. 2-6 The "alkenyl" has a similar explanation, except that the number of carbon atoms is different.
[0071] "Substituted or unsubstituted C2~30 "Alkynyl" means a straight or branched hydrocarbon group having one or more triple bonds, and the total number of carbon atoms in the group is 2 to 30. The triple bonds in the group can be in any position, and the optional C 2~30 At least one H in the alkynyl group is substituted by a corresponding group as defined herein. 2-10 The "alkynyl group" has a similar interpretation, except that the number of carbon atoms is different.
[0072] "Substituted or unsubstituted C 6~30 "Aryl" means an all-carbon monocyclic or fused polycyclic group having a completely conjugated π electron system. "Aryl" means an all-carbon monocyclic or fused polycyclic group having 6 to 30 carbon atoms; for example, benzene, naphthalene, indene, fluorene, etc. and optionally C 6~30 At least one H in the aryl group is substituted by a corresponding group as defined herein. 6-15 The "aryl group" has a similar explanation, except that the number of carbon atoms is different.
[0073] "Substituted or unsubstituted C 6~30 "heteroaryl" means a monocyclic or fused ring group of ring atoms, containing one, two, three or four ring heteroatoms selected from N, O or S, the remaining ring atoms are C, and further has a completely conjugated π electron system, a total carbon number of 6 to 30, and optionally C 6~30 At least one H in the heteroaryl group is substituted by a corresponding group as defined herein. 6-15 The "heteroaryl" has a similar explanation, except that the number of carbon atoms is different.
[0074] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0075] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0076] Figure 1 It is a schematic diagram of the structure of a solar cell device of the present invention;
[0077] Figure 2 The JV curve diagram of the organic acceptor materials prepared in Example 1 and Example 2 applied to organic solar cells;
[0078] Figure 3 This is an EQE curve diagram of the organic acceptor materials prepared in Example 1 and Example 2 applied to organic solar cells. DETAILED DESCRIPTION
[0079] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0080] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0081] Example 1
[0082] Example 1 provides an organic receptor material, and its reaction equation and preparation method are as follows:
[0083]
[0084] S1. In a 250mL round-bottom flask, weigh 2-amino-3,6-dibromobenzenethiol (5g, 17.6mmol), isooctylaldehyde (3.1g, 21.2mmol) and hexadecyltrimethylammonium bromide in an aqueous solution and stir to react for 24h. After the reaction, extract with dichloromethane, spin dry the solvent to obtain a crude product, separate and purify with silica gel column chromatography to obtain a solid product, namely compound 2 (4.65g, 65%); HRMS (m / z, MALDI): Calc.for C 15 H 19 BrNS, [M+H]+: 405.19, found: 404.96.
[0085] S2. Add compound 2 (4 g, 9.8 mmol) to a 250 mL round-bottom flask equipped with a stirring bar and dissolve it in concentrated sulfuric acid (40 mL), then add concentrated nitric acid. After a period of reaction, add concentrated sulfuric acid and potassium nitrate, and then reflux for 24 h. Dry tetrahydrofuran and extract with dichloromethane. Dry the solvent to obtain a crude product, separate and purify it with silica gel column chromatography to obtain a solid product, namely compound 3 (3.32 g, 68%); HRMS (m / z, MALDI): Calc.for C 15 H 17 Br2N3O4S, [M+H]+: 495.19, found: 494.93.
[0086] S3. In a 250 mL round-bottom flask, weigh compound 3 (3 g, 6.1 mmol) and tributyl (5-phenylhexyl-thieno [3, 2-b] thiophene-2-yl) stannane (7.85 g, 13.3 mmol) and dissolve them in 80 mL toluene, replace the gas, pass argon for 15 minutes, and add tetrakis (triphenylphosphine) palladium Pd (PPh3) 4 (0.17 g, 0.14 mmol) to the reaction system under argon protection. The reactants were refluxed at 110 ° C for 24 hours. Cool to room temperature, spin dry toluene, extract with dichloromethane, spin dry the solvent to obtain a crude product, separate and purify by silica gel column chromatography to obtain a red solid, which is compound 5 (4.60 g, 80%); HRMS (m / z, MALDI): Calc.for: C 51 H 71 N3O4S5,[M+H] + :950.45, found:949.40.
[0087] S4. Add compound 5 (2 g, 2.11 mmol) and triethyl phosphite (10 mL) to a 250 mL sealed tube, dissolve in anhydrous 1,2-dichlorobenzene (o-DCB, 10 mL), and stir the mixture at 180 ° C overnight. After the reaction is completed and cooled to room temperature, the solvent is removed by distillation under reduced pressure to obtain a red intermediate. Subsequently, the red intermediate is mixed with K2CO3 (2.70 g, 19.5 mmol), KI (0.32 g, 1.95 mmol), 2-butyl-1-bromooctane (1.46 g, 5.85 mmol) and anhydrous DMF (25 mL) and stirred overnight at 100 ° C under argon atmosphere. After the reaction is completed, the reaction mixture is extracted with ethyl acetate 3 times and the organic phase is washed with brine. The organic phase is then dried over Na2SO4 and evaporated under reduced pressure to obtain an orange oil. Then, petroleum ether / dichloromethane (6 / 1, v / v) was used as the eluent to obtain compound 6 (1.66 g, 71%) by silica gel column chromatography; HRMS (m / z, MALDI): Calc.for: C 67 H 103 N3S5, [M+H]+: 1110.88, found: 1111.68.
[0088] S5. Add compound 6 (0.50 g, 0.45 mmol) and anhydrous N,N-formamide (25 mL) to a 100 mL three-necked flask, stir at 0°C for a few minutes, and then add phosphorus oxychloride (1.5 mL). After stirring the reaction solution at 0°C for 1 hour, raise the temperature to 90°C and stir overnight, cool to room temperature, extract with dichloromethane, spin dry the solvent, and separate and purify by silica gel column chromatography to obtain compound 7 (0.43 g, 82%); HRMS (m / z, MALDI): Calc.for: C 69 H103 N3O2S5,[M+H]+: 1166.90, found: 1165.67.
[0089] S6. In a 100 mL round-bottom flask, compound 7 (300 mg, 0.26 mmol) and 5,6-difluoro-3-(dicyanomethylidene)indone (389.2 mg, 1.01 mmol) were dissolved in 50 mL of chloroform, and the gas was replaced three times. Under argon protection, 2.5 mL of pyridine was slowly added while stirring. The mixture was refluxed under argon protection for 12 h, cooled to room temperature, poured into 300 mL of anhydrous methanol, and filtered to obtain a crude product. The product was separated and purified by silica gel column chromatography to obtain a dark blue solid, namely (PhNSB-4F) (278.3 mg, 68%), HRMS (m / z, MALDI): Calc.for: C 97 H 107 F4N7O2S5,[M+H] + :1591.22, found:1592.71.
[0090] Example 2
[0091] Example 2 provides an organic receptor material, and its reaction equation and preparation method are as follows:
[0092]
[0093] S6. Compound 7 (300 mg, 0.26 mmol) in Example 1 and 5,6-dichloro-3-(dicyanomethylidene)indone (400 mg, 1.52 mmol) were dissolved in 50 mL of chloroform, and the gas was replaced three times. Under argon protection, 2.5 mL of pyridine was slowly added while stirring. The mixture was refluxed under argon protection for 12 h, cooled to room temperature, poured into 300 mL of anhydrous methanol, and filtered to obtain a crude product. The crude product was separated and purified by silica gel column chromatography to obtain a dark blue solid, namely (PhNSB-4Cl) (231.9 mg, 73%), HRMS (m / z, MALDI): Calc.for: C 97 H 107 Cl4N7O2S5[M+H] + :1657.58,found:1657.39.
[0094] Performance Testing
[0095] The preparation and characterization of organic photovoltaic (OPV) devices are as follows:
[0096] like Figure 1As shown, the OPV device includes a substrate, a hole transport layer, an active layer, an electron transport layer and a metal electrode in sequence. The commercially purchased indium tin oxide (ITO) glass substrate (specification: 1.5cm*1.5cm) is first scrubbed with acetone, then ultrasonically cleaned with detergent, water, deionized water, acetone, and isopropanol in sequence, and then dried and spin-coated with a 30nm thick PEDOT:PSS layer as a hole transport layer for standby use. The polymer donor material PM6, L8-BO and PhNSB-4F or PhNSB-4Cl prepared in Example 1 or 2 (weight ratio of 1:1.1:0.1) and the additive chloronaphthalene (0.25%-3%) in chlorobenzene mixed solution (10-30mg / mL) are spin-coated on the PEDOT:PSS hole transport layer to form the ternary active layer of the device. Finally, a layer of PNDIT-F3N with a thickness of about 10 nm was spin-coated as an electron transport layer and Ag (100 nm) was used as a device metal electrode to obtain a solar cell device cell structure: ITO / PEDOT:PSS / active layer / PNDIT-F3N / Ag).
[0097] The structures of the polymer donor materials PM6 and L8-BO (purchased from Shuo Lun Organic Photoelectric Technology (Beijing) Co., Ltd.) and the electron transport layer PNDIT-F3N (purchased from Nanjing Zhiyan Technology Co., Ltd.) used in the above-mentioned organic solar cell device are as follows:
[0098]
[0099] The energy conversion efficiency of solar cells is calculated using Guangyan SS-F5-3A as a solar simulator at 100mW / cm 2 The photovoltaic performance of the device was tested under light intensity, and the light intensity was calibrated by a standard single-crystal silicon solar cell (SRC-00019); the JV curve was measured using Keithley 2400. The open circuit voltage, short circuit current and fill factor of the above solar cell device were obtained from the test, and the corresponding photoelectric conversion efficiency was calculated.
[0100] The JV curve of a solar cell device is as follows: Figure 2 As shown, the open circuit voltage V of the solar cell device with PhNSB-4F as the third component of the active layer OC =0.86V, short circuit current J SC =26.9mA / cm 2 , fill factor FF = 76.45%, conversion efficiency PCE = 17.58%; the open circuit voltage V OC =0.87V, short circuit current J SC =25.07mA / cm 2, filling factor FF = 79.60%, conversion efficiency PCE = 17.39%.
[0101] Figure 3 EQE curves of PhNSB-4F and PhNSB-4Cl in Examples 1 and 2 when applied to organic solar cells. The integrated short-circuit currents obtained according to the EQE curves are 24.50 mA / cm 2 and 24.05mA / cm 2 , which is within 5% of the test value, indicating that the device data is highly reliable.
[0102] The preparation and characterization of large-area printed OPV devices are as follows:
[0103] 20cm 2 The IT0 conductive glass is then ultrasonically cleaned with detergent, water, deionized water, acetone, and isopropanol in turn. After drying, a 30nm thick PEDOT:PSS layer is spin-coated on the substrate as a hole transport layer for standby use. The polymer donor material PM6 and the acceptor material prepared in L8-BO or Example 1 (weight ratio of 1:1.3), as well as the additive chloronaphthalene (0.25%) in chloroform (10-30mg / mL) are printed on the PEDOT:PSS layer to form an active layer thickness of 300nm. PNDIT-F3N is dissolved in methanol solution and 0.5% acetic acid is added to prepare a 1moL / mL solution. The solution is spin-coated on the surface of the active layer at a speed of 4000 revolutions per second, and then annealed at 100°C for 10min to prepare an electron transport layer with a thickness of 8nm. Finally, the Ag electrode is prepared by printing technology, and silver paste is used as the raw material. A layer of silver paste is directly brushed on the surface of the prepared electron transport layer as an electrode, and the thickness of the electrode layer is 100 nm.
[0104] Performance test of large-area devices: select a large-area battery for testing under standard test conditions: AM1.5, 100mW / cm 2 The open circuit voltage (V OC )=0.83V, short circuit current (J SC )=22.16mA / cm2, fill factor (FF)=0.51, photoelectric conversion efficiency (PCE)=9.37%. At the same time, the open circuit voltage (VOC) of the Y6 device is 0.69V, the short circuit current (J SC )=20.27mA / cm2, fill factor (FF)=0.39, photoelectric conversion efficiency (PCE)=5.44%.
[0105] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. An organic receptor material, characterized in that Including compounds having formula (I); ; Wherein, R1 and R3 are independently selected from C 1~30 Branched alkyl; R2 is selected from one of the following structural formulas: ; Wherein, R4 is selected from C 1~30 A straight chain alkyl group; A1 and A2 are selected from the following structural formulas: ; wherein X1 and X2 are independently selected from halogen.
2. The organic receptor material according to claim 1, characterized in that The compound I is selected from one of the following structural formulas: 、 。 3. The method for preparing an organic receptor material according to claim 1 or 2, characterized in that: The steps include: S6, adding compound 7, compound A1 or A2, a first organic solvent and pyridine, and obtaining an organic acceptor material by Knoevenagel reaction under an inert gas; 。 4. The method for preparing an organic receptor according to claim 3, characterized in that: The first organic solvent is selected from at least one of chloroform, toluene and chlorobenzene.
5. Use of the organic acceptor material according to claim 1 or 2 in solar cells.
6. A solar cell active layer, comprising an acceptor material and a polymer donor, characterized in that: The acceptor material is selected from the organic acceptor material according to claim 1 or 2.
7. The solar cell active layer according to claim 6, characterized in that: The polymer donor is selected from at least one of PM6, PBDB-T, D18, and PTQ-10.
8. An organic solar cell, characterized in that: It comprises a substrate, a hole transport layer, an active layer, an electron transport layer and a metal electrode in sequence; the active layer is selected from the solar cell active layer according to claim 6 or 7.