Wave-absorbing sheaths and their applications in cables

By using a wave-absorbing sheath made of composite magnetic material, the problem of poor electromagnetic interference suppression in cables is solved, achieving good electromagnetic interference suppression and durability, making it suitable for cable applications.

CN116390465BActive Publication Date: 2026-11-17ZHEJIANG DAHUA TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310418346.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2026-11-17
Estimated Expiration
2043-04-14

AI Technical Summary

Technical Problem

Existing cables have poor electromagnetic interference suppression, and ferrite cores are difficult to fit completely with the cables. They are also fragile, inconvenient to install, and have a limited lifespan.

Method used

The wave-absorbing sheath, made of composite magnetic materials including porous graphene ellipsoids, zinc sulfide nanomaterials, and tungsten carbide nanomaterials, has excellent wave-absorbing performance and flexibility. When used with nested cables, it enhances the electromagnetic interference suppression effect.

Benefits of technology

The absorbing sheath fits the cable well, effectively suppresses electromagnetic interference, is easy to install, does not increase the size and weight of the cable, is resistant to vibration and transportation damage, and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116390465B_ABST
    Figure CN116390465B_ABST
Patent Text Reader

Abstract

This invention relates to a microwave absorbing sheath and its application in cables. The raw materials for preparing the microwave absorbing sheath include a composite magnetic material and a coagulant. The composite magnetic material comprises a composite material composed of porous graphene ellipsoids, zinc sulfide nanomaterials, and tungsten carbide nanomaterials, and an organic insulating material coating the surface of the composite material. In the composite material, multiple porous graphene ellipsoids are arranged in an orderly manner to form a graphene cluster, and the zinc sulfide nanomaterials and tungsten carbide nanomaterials are fused within the graphene cluster. The microwave absorbing sheath of this invention has excellent microwave absorption performance and is also lightweight, thin, and flexible. Therefore, the microwave absorbing sheath of this invention can be nested within cables, providing better fit and suppression of electromagnetic interference. It is also easy to install without increasing the size and weight of the cable, and will not damage the cable due to unavoidable factors such as vibration or transportation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electromagnetic absorbing materials technology, and in particular to absorbing sheaths and their application in cables. Background Technology

[0002] With the rapid development of electronic information technology, high-power, high-speed electronic devices are moving towards high integration and miniaturization. However, as the degree of integration increases and the size decreases, electromagnetic radiation interference is inevitable. This not only harms human health, but also causes electromagnetic interference generated inside electronic devices. This interference is radiated to the outside world along with the antenna formed by external cables or the crosstalk between connecting cables and audio / video cables between the PCBs of the device, or it can directly affect the inside of the device.

[0003] Currently, most cables use ferrite cores to suppress electromagnetic interference. However, electronic equipment cables vary widely in size and diameter, making it difficult for ferrite cores to fit perfectly with the cables. Gaps can occur during assembly, leading to electromagnetic wave leakage and reduced suppression effectiveness. Furthermore, ferrite is a rigid material lacking flexibility and ductility, making it brittle. This not only makes installation inconvenient but also increases the size and weight of the cables. Moreover, after installing ferrite cores, unavoidable factors such as vibration and transportation can damage the cables, reducing their lifespan. Summary of the Invention

[0004] Therefore, it is necessary to provide a wave-absorbing sheath and its application in cables to address the above-mentioned technical problems. The wave-absorbing sheath not only has excellent wave-absorbing performance, but also has the characteristics of being light, thin, and flexible, and can be used to nest cables to better suppress electromagnetic interference.

[0005] The present invention provides a microwave absorbing sheath, wherein the raw materials for preparing the microwave absorbing sheath include composite magnetic materials and a coagulant;

[0006] The composite magnetic material includes a composite material composed of porous graphene ellipsoids, zinc sulfide nanomaterials and tungsten carbide nanomaterials, and an organic insulating material coated on the surface of the composite material. In the composite material, multiple porous graphene ellipsoids are arranged in an orderly manner to form a graphene group, and the zinc sulfide nanomaterials and the tungsten carbide nanomaterials are fused into the graphene group.

[0007] In one embodiment, the composite magnetic material has a mass fraction of 50%-70% in the microwave absorbing sheath.

[0008] In one embodiment, the porous graphene ellipsoids in the graphene group are arranged in a three-dimensional array.

[0009] In one embodiment, the porous graphene ellipsoid has an equatorial radius of 100nm-120nm and a polar radius of 200nm-250nm.

[0010] In one embodiment, the pore size of the porous graphene ellipsoid is 14nm-25nm.

[0011] In one embodiment, the ratio of the particle size of the zinc sulfide nanomaterial to the pore size of the porous graphene ellipsoid is 1:8 to 1:12.

[0012] In one embodiment, the mass ratio of the zinc sulfide nanomaterial to the graphene group in the composite magnetic material is 1:3-1:5.

[0013] In one embodiment, the ratio of the particle size of the tungsten carbide nanomaterial to the pore size of the porous graphene ellipsoid is 1:9 to 1:15.

[0014] In one embodiment, the mass ratio of the tungsten carbide nanomaterial to the graphene group in the composite magnetic material is 1:4-1:7.

[0015] The present invention also provides an application of the aforementioned absorbing sheath in cables.

[0016] This invention, through the selection of materials and the control of structure in the composite magnetic material, achieves an insertion loss of approximately 30% in the 0.15MHz-30MHz frequency band, exhibiting excellent microwave absorption performance. Furthermore, the composite magnetic material of this invention uses a graphene swarm composed of multiple porous graphene ellipsoids arranged in an orderly manner as the matrix, incorporating zinc sulfide nanomaterials and tungsten carbide nanomaterials. This results in a dense structure, good toughness, and resistance to breakage under load, exhibiting excellent ductility. Furthermore, when mixed with a coagulant, the resulting microwave absorbing sheath is lightweight, thin, and flexible.

[0017] Therefore, the absorbing sheath of the present invention can be nested with cables, has better fit with cables, can better suppress electromagnetic interference, and is easy to install without increasing the size and weight of the cables, and will not damage the cables due to unavoidable factors such as vibration and transportation. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 This is a high-magnification scanning electron microscope image of the graphene group obtained in Example 1;

[0020] Figure 2 This is a high-magnification scanning electron microscope image of the composite magnetic material prepared in Example 1;

[0021] Figure 3 Electromagnetic compatibility (EMC) conducted interference diagram for network cables;

[0022] Figure 4 The electromagnetic compatibility conducted interference diagram is shown after the absorbing sheath of the network cable in Example 1. Detailed Implementation

[0023] To facilitate understanding of the present invention, it will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. Rather, these embodiments or examples are provided to make the disclosure of the present invention more thorough and complete.

[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments or examples only and is not intended to limit the invention. The optional scope of the term "and / or" as used herein includes any one of two or more of the related listed items, as well as any and all combinations of the related listed items, including any two related listed items, any more related listed items, or a combination of all related listed items.

[0025] The raw materials for preparing the microwave absorbing sheath provided by the present invention include composite magnetic materials and a coagulant; wherein, the composite magnetic material includes a composite material composed of porous graphene ellipsoids, zinc sulfide nanomaterials and tungsten carbide nanomaterials, and an organic insulating material coating the surface of the composite material, wherein, in the composite material, multiple porous graphene ellipsoids are arranged in an orderly manner to form a graphene group, and the zinc sulfide nanomaterials and the tungsten carbide nanomaterials are fused into the graphene group.

[0026] Specifically, the zinc sulfide nanomaterials are integrated into the graphene group in the following ways: zinc sulfide nanomaterials are attached to the surface of at least a portion of the porous graphene ellipsoids, and zinc sulfide nanomaterials are filled in at least a portion of the gaps in the graphene group; furthermore, when the particle size of the zinc sulfide nanomaterials is smaller than the pore size of the porous graphene ellipsoids, the integration of the zinc sulfide nanomaterials into the graphene group also includes the presence of zinc sulfide nanomaterials within the channels of at least a portion of the porous graphene ellipsoids. Of course, the specific integration method will not have a substantial impact on the wave absorption performance.

[0027] Similarly, the tungsten carbide nanomaterials are integrated into the graphene group in the following ways: at least a portion of the porous graphene ellipsoids are coated with tungsten carbide nanomaterials, and at least a portion of the gaps in the graphene group are filled with tungsten carbide nanomaterials; furthermore, when the particle size of the tungsten carbide nanomaterials is smaller than the pore size of the porous graphene ellipsoids, the tungsten carbide nanomaterials are integrated into the graphene group in the following ways: at least a portion of the porous graphene ellipsoids contain tungsten carbide nanomaterials within their pores. Of course, the specific integration method will not have a substantial impact on the wave absorption performance.

[0028] Different structural types and materials exhibit varying electromagnetic wave conversion capabilities. In this invention, graphene, zinc sulfide, and tungsten carbide are used in combination. Structurally, graphene particles are bonded together with binders such as phenolic resin to form porous graphene ellipsoids, which are then arranged in an orderly manner to form graphene clusters. Zinc sulfide nanomaterials and tungsten carbide nanomaterials are integrated into these graphene clusters in various ways. This allows for faster and more efficient conversion of electromagnetic waves into heat energy. Furthermore, graphene's excellent thermal conductivity enables rapid heat transfer, resulting in a composite magnetic material with an insertion loss of approximately 30% in the 0.15MHz-30MHz frequency band, demonstrating excellent wave absorption performance.

[0029] Meanwhile, the composite magnetic material of this invention uses a graphene cluster composed of multiple porous graphene ellipsoids arranged in an orderly manner as the matrix, and integrates zinc sulfide nanomaterials and tungsten carbide nanomaterials. It exhibits a dense structure, good toughness, and is not prone to breakage under load, thus possessing excellent ductility. Furthermore, graphene, zinc sulfide, and tungsten carbide have low densities, and the composite material is coated with an organic insulating material, which not only gives the composite magnetic material insulation but also makes the bonding of the composite material more stable. Moreover, after the composite magnetic material is mixed with a coagulant, the resulting microwave absorbing sheath is lightweight, thin, and flexible.

[0030] Optionally, during the coating process, the organic insulating material can partially coat the surface of the composite material or completely coat the composite material. Preferably, the organic insulating material completely coats the composite material. The organic insulating material is preferably a block polymer, such as ethylene oxide and propylene oxide block copolymer ether.

[0031] To further optimize the absorption performance and flexibility of the absorbing sheath, composite magnetic materials can be further optimized.

[0032] For example, in composite magnetic materials, when multiple porous graphene ellipsoids are arranged in an orderly manner to form a graphene group, the porous graphene ellipsoids are arranged in a three-dimensional array; and / or, the equatorial radius of the porous graphene ellipsoids is 100nm-120nm, including but not limited to 100nm, 105nm, 110nm, 115nm, 120nm, etc., and the polar radius is 200nm-250nm, including but not limited to 200nm, 205nm, 210nm, 215nm, 220nm, 225nm, 230nm, 235nm, 240nm, 245nm, 250nm, etc.; and / or, the pore size of the porous graphene ellipsoids is 1 The particle size distribution is 4nm-25nm, including but not limited to 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, 20nm, 21nm, 22nm, 23nm, 24nm, 25nm, etc., and the ratio of the particle size of the zinc sulfide nanomaterial to the pore size of the porous graphene ellipsoid is 1:8-1:12, including but not limited to 1:8, 1:9, 1:10, 1:11, 1:12, etc.; and / or, the ratio of the particle size of the tungsten carbide nanomaterial to the pore size of the porous graphene ellipsoid is 1:9-1:15, including but not limited to 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, etc.

[0033] For example, the mass ratio of porous graphene ellipsoids, zinc sulfide nanomaterials, and tungsten carbide nanomaterials in the composite magnetic material can be further optimized. In one embodiment, the mass ratio of zinc sulfide nanomaterials to graphene groups in the composite magnetic material is 1:3-1:5, including but not limited to 1:3, 1:4, 1:5, etc.; and / or, the mass ratio of tungsten carbide nanomaterials to graphene groups is 1:4-1:7, including but not limited to 1:4, 1:5, 1:6, 1:7, etc.

[0034] In one embodiment, the composite magnetic material has a mass fraction of 50%-70% in the microwave absorbing sheath, which is also beneficial for optimizing the microwave absorbing performance and flexibility of the microwave absorbing sheath.

[0035] In the microwave absorbing sheath, the choice of coagulant material does not affect its microwave absorption effect. The present invention does not restrict the choice of coagulant. Preferably, the coagulant is selected from propylene glycol, disodium ethylenediaminetetraacetate, disodium stannous citrate, glucono-δ-lactone and insoluble polyvinylpyrrolidone, etc.

[0036] It should be noted that the size and diameter of the absorbing sheath of the present invention can be selected according to the size and diameter of the cable, and the thickness and shape of the sheath are not limited.

[0037] The preparation method of the microwave absorbing sheath of the present invention is not limited. In one embodiment, the preparation method of the microwave absorbing sheath includes the following steps: mixing composite magnetic material with coagulant to obtain slurry, then placing the slurry in a mold, and obtaining the microwave absorbing sheath after curing.

[0038] To ensure better mixing of the composite magnetic material and the coagulant, the composite magnetic material can be mixed with water first, and then mixed with the coagulant.

[0039] This invention does not limit the preparation method of composite magnetic materials; any preparation method can be used to obtain them, as long as the structure and materials meet the above-mentioned conditions of this invention, the desired effect can be achieved.

[0040] In one embodiment, the preparation method of the composite magnetic material includes the following steps: preparing graphene groups using a colloidal crystal template method, then mixing the graphene groups with zinc sulfide nanomaterials, adding organic insulating materials, heating to a viscous state, and then cooling to obtain the composite magnetic material.

[0041] The specific steps for preparing graphene groups using the colloidal crystal template method include: preparing a first formulation by mixing graphene with water, then mixing the first formulation with a binder to form a second formulation, then adding the second formulation to a colloidal crystal template and heating it under an inert atmosphere, and then cooling it under a reducing atmosphere to obtain graphene groups.

[0042] The graphene to water mass ratio is 1:2-1:4, the graphene to binder mass ratio is 10:1-10:3, the binder is preferably a resin-based binder, such as phenolic resin, the graphene to colloidal crystal mass ratio is 6:1-12:1, the colloidal crystal template is selected from polymethyl methacrylate colloidal crystal template, the heating temperature is preferably 180℃-220℃, the heating time is preferably 20h-28h, the inert atmosphere is selected from nitrogen, argon, etc., and the reducing atmosphere is selected from carbon monoxide, hydrogen, etc.

[0043] To further improve the stability of graphene, a reducing catalyst, such as SnCl2 or FeCl2, can be added to the first formulation. The mass ratio of graphene to the reducing catalyst is 1:1 to 2:1. Then, the mixture is heated in an inert gas and cooled in a reducing atmosphere to obtain a more stable first formulation. The preferred heating temperature is 220℃ to 280℃, and the preferred heating time is 4h to 8h.

[0044] This invention also provides an application of the aforementioned absorbing sheath in cables. Because the absorbing sheath of this invention has excellent absorption performance, and is also lightweight, thin, and flexible, it can be nested within cables, providing better fit and suppression of electromagnetic interference. Furthermore, it is easy to install without increasing the size and weight of the cable, and it prevents damage to the cable due to unavoidable factors such as vibration and transportation.

[0045] The following specific examples will further illustrate the absorbing sheath and its application in cables.

[0046] Example 1

[0047] Graphene powder was added to water at a mass ratio of 1:3 and mixed. Then, SnCl2 was added at a mass ratio of 1:1 to the graphene powder. The mixture was placed in an argon atmosphere and heated at 250°C for 6 hours, followed by cooling in a CO atmosphere to obtain the first formulation. The first formulation was then mixed with phenolic resin to obtain the second formulation, wherein the mass ratio of graphene powder to phenolic resin was 10:2.

[0048] The second formulation was added to polymethyl methacrylate colloidal crystals at a mass ratio of graphene to polymethyl methacrylate colloidal crystals of 8:1. The mixture was then placed in an argon atmosphere and heated at 200°C for 24 hours, followed by cooling in a carbon monoxide atmosphere to obtain the desired product. Figure 1 The graphene group shown is composed of porous graphene ellipsoids arranged in a three-dimensional array. The equatorial radius of the porous graphene ellipsoids is 100 nm, the polar radius is 210 nm, and the pore size is 18 nm.

[0049] Graphene groups, zinc sulfide nanomaterials with a particle size of 1.8 nm, and tungsten carbide nanomaterials with a particle size of 2 nm were added to water, with the mass ratio of graphene groups to zinc sulfide nanomaterials being 4:1 and the mass ratio of graphene groups to tungsten carbide nanomaterials being 5:1. The mixture was stirred and mixed, then ethylene oxide and propylene oxide block copolymer ethers were added, and the mixture was placed in an argon atmosphere and heated to 150°C until it reached a viscous state. After cooling, the mixture was obtained as shown in the figure. Figure 2 The composite magnetic material shown.

[0050] The composite magnetic material is dispersed in water, and then sodium stannous citrate is added to obtain a slurry, wherein the mass ratio of the composite magnetic material to sodium stannous citrate is 2:1.

[0051] A mold is provided, the above slurry is poured into the mold, and after curing, a microwave absorbing sheath is obtained.

[0052] Example 2

[0053] Example 2 was carried out in accordance with Example 1, except that the mass ratio of graphene group to zinc sulfide nanomaterial was 5:1, and the mass ratio of graphene group to tungsten carbide nanomaterial was 6:1.

[0054] Example 3

[0055] Example 3 was carried out in accordance with Example 1, except that the mass ratio of graphene group to zinc sulfide nanomaterial was 3:1, and the mass ratio of graphene group to tungsten carbide nanomaterial was 7:1.

[0056] Example 4

[0057] Example 4 was carried out in accordance with Example 1, except that the second formulation was added to polymethyl methacrylate colloidal crystals and heated at 180°C for 24 hours. The equatorial radius of the porous carbon rod was 100 nm, the polar radius was 200 nm, and the pore diameter was 14 nm. In addition, the particle size of the zinc sulfide nanomaterial was 1.7 nm, and the particle size of the tungsten carbide nanomaterial was 1.2 nm.

[0058] Example 5

[0059] Example 5 was carried out in accordance with Example 1, except that the second formulation was added to polymethyl methacrylate colloidal crystals and heated at 220°C for 22 hours. The equatorial radius of the porous carbon rod was 110 nm, the polar radius was 210 nm, and the pore diameter was 17 nm. In addition, the particle size of the zinc sulfide nanomaterial was 1.7 nm, and the particle size of the tungsten carbide nanomaterial was 1.2 nm.

[0060] Example 6

[0061] Example 6 was carried out in accordance with Example 1, except that the second formulation was added to polymethyl methacrylate colloidal crystals and heated at 220°C for 24 hours. The equatorial radius of the porous carbon rod was 120 nm, the polar radius was 220 nm, and the pore diameter was 22 nm. In addition, the particle size of zinc sulfide nanomaterials was 2 nm, and the particle size of tungsten carbide nanomaterials was 2 nm.

[0062] Example 7

[0063] Example 7 was carried out in accordance with Example 1, except that the mass ratio of the composite magnetic material to sodium stannous citrate was 1:1.

[0064] Example 8

[0065] Example 8 was carried out in accordance with Example 1, except that the mass ratio of the composite magnetic material to sodium stannous citrate was 2.3:1.

[0066] Comparative Example 1

[0067] Comparative Example 1 was carried out in accordance with Example 1, except that tungsten carbide nanomaterials were not added.

[0068] Comparative Example 2

[0069] Comparative Example 2 was carried out in accordance with Example 1, except that zinc sulfide nanomaterials were not added.

[0070] Comparative Example 3

[0071] Comparative Example 3 was carried out in accordance with Example 1, except that the second formulation was added to polymethyl methacrylate colloidal crystals and heated at 150°C for 24 hours to obtain a three-dimensional arrangement of spherical graphene groups.

[0072] Comparative Example 4

[0073] Comparative Example 4 was carried out in accordance with Example 1, except that the second formulation was added to polymethyl methacrylate colloidal crystals and heated at 190°C for 18 hours to obtain a three-dimensional arrangement of rod-shaped graphene groups.

[0074] Comparative Example 5

[0075] Comparative Example 5 was carried out in accordance with Example 1, except that carbon nanotubes were used instead of graphene to obtain a group of carbon nanotubes arranged in three dimensions of porous carbon nanotube ellipsoids.

[0076] The microwave absorption performance of the microwave absorbing sheaths obtained in Examples 1-8 and Comparative Examples 1-5 was tested. The test methods are shown below, and the test results are shown in Table 1.

[0077] Absorption performance: Refer to GB / T32596 to test absorption bandwidth and insertion loss.

[0078] Flexibility: Measured according to ASTM F147-1987 (2017).

[0079] Table 1

[0080] Absorption bandwidth / MHz Insertion loss / dB Extension range / mm Example 1 0.15-30 27-33 2-3 Example 2 0.15-30 26-33 2-3 Example 3 0.15-30 25-31 2-3 Example 4 0.17-30 24-30 2-3 Example 5 0.19-30 26-30 2-3 Example 6 0.2-30 23-29 2-3 Example 7 0.15-30 24-30 2-4 Example 8 0.15-30 28-33 1.5-3 Comparative Example 1 30-1000 19-26 2-2.5 Comparative Example 2 0.15-30 16-21 1.5-2.5 Comparative Example 3 3000-10000 12-17 2-2.5 Comparative Example 4 3000-10000 15-19 2-2.5 Comparative Example 5 3000-10000 12-16 2-2.5

[0081] Application Experiment

[0082] Electromagnetic compatibility conducted interference tests were performed on the network cable, and the results are as follows: Figure 3As shown, the absorbing sheath prepared in Example 1 was then nested into the network cable, and electromagnetic compatibility conducted interference tests were performed. The results are as follows. Figure 4 As shown, comparison Figure 3 and Figure 4 It is understood that the electromagnetic interference can be effectively suppressed after the absorbing sheath of the present invention is nested.

[0083] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0084] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A microwave absorbing sheath, characterized in that, The raw materials for preparing the microwave absorbing sheath include composite magnetic materials and a coagulant; The composite magnetic material comprises a composite material composed of porous graphene ellipsoids, zinc sulfide nanomaterials, and tungsten carbide nanomaterials, and an organic insulating material coating the surface of the composite material. In the composite material, the mass ratio of zinc sulfide nanomaterials to graphene groups is 1:3-1:5, and the mass ratio of tungsten carbide nanomaterials to graphene groups is 1:4-1:

7. Multiple porous graphene ellipsoids are arranged in an orderly manner to form graphene groups. The zinc sulfide nanomaterials and tungsten carbide nanomaterials are fused into the graphene groups. The equatorial radius of the porous graphene ellipsoids is 100nm-120nm, and the polar radius is 200nm-250nm.

2. The microwave absorbing sheath according to claim 1, characterized in that, The composite magnetic material has a mass fraction of 50%-70% in the microwave absorbing sheath.

3. The microwave absorbing sheath according to claim 1 or 2, characterized in that, In the graphene group, the porous graphene ellipsoids are arranged in a three-dimensional array.

4. The microwave absorbing sheath according to claim 1 or 2, characterized in that, The zinc sulfide nanomaterial is integrated into the graphene group in the following ways: the zinc sulfide nanomaterial is attached to the surface of at least a portion of the porous graphene ellipsoids, and the zinc sulfide nanomaterial is filled in at least a portion of the gaps in the graphene group. When the particle size of the zinc sulfide nanomaterial is smaller than the pore size of the porous graphene ellipsoids, the integration of the zinc sulfide nanomaterial into the graphene group further includes the zinc sulfide nanomaterial being contained within the channels of at least a portion of the porous graphene ellipsoids. And / or, the tungsten carbide nanomaterial is integrated into the graphene group in the following ways: at least a portion of the surface of the porous graphene ellipsoids is coated with the tungsten carbide nanomaterial, and at least a portion of the gaps in the graphene group is filled with the tungsten carbide nanomaterial. When the particle size of the tungsten carbide nanomaterial is smaller than the pore size of the porous graphene ellipsoids, the tungsten carbide nanomaterial is integrated into the graphene group in the following ways: at least a portion of the channels of the porous graphene ellipsoids contain the tungsten carbide nanomaterial.

5. The microwave absorbing sheath according to claim 1 or 2, characterized in that, The porous graphene ellipsoid has a pore size of 14nm-25nm.

6. The microwave absorbing sheath according to claim 5, characterized in that, The ratio of the particle size of the zinc sulfide nanomaterial to the pore size of the porous graphene ellipsoid is 1:8 to 1:

12.

7. The microwave absorbing sheath according to claim 5, characterized in that, The ratio of the particle size of the tungsten carbide nanomaterial to the pore size of the porous graphene ellipsoid is 1:9-1:

15.

8. The microwave absorbing sheath according to claim 1 or 2, characterized in that, In the composite magnetic material, the coagulant is selected from at least one of propylene glycol, disodium ethylenediaminetetraacetate, disodium stannous citrate, glucono-δ-lactone, or insoluble polyvinylpyrrolidone.

9. A method for preparing a microwave absorbing sheath as described in any one of claims 1-8, characterized in that, Includes the following steps: The composite magnetic material is mixed with a coagulant to obtain a slurry, which is then placed in a mold and cured to obtain a microwave absorbing sheath.

10. An application of the absorbing sheath as described in any one of claims 1-8 in a cable.

Citation Information

Patent Citations

  • Flexible graphene film and flexible graphene-based composite material film as well as preparation methods thereof

    CN107500271A

  • Three-dimensional ordered porous graphene wave-absorbing material and preparation method thereof

    CN113511648A

  • Communication cable

    JP1999111077A