A near-zero carbon emission prefabricated building insulation board and preparation method
By using slag and magnesium slag to prepare foam concrete, combined with sodium bicarbonate and alum foaming agents and phosphogypsum, the problems of low maintenance efficiency of inorganic insulation materials and fire hazards of organic materials are solved, achieving high performance and low carbon emissions. Prefabricated building insulation panels have excellent fire protection, heat insulation and pressure resistance properties.
Patent Information
- Application Number
- CN202310196884.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-03
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-03-03
AI Technical Summary
Existing inorganic insulation materials have low carbon dioxide curing efficiency and are difficult to meet the needs of large-sized components, and organic insulation materials have problems such as fire hazards and poor durability.
Foam concrete is prepared using slag and magnesium slag as cementitious materials, combined with sodium bicarbonate and alum as foaming agents to generate carbon dioxide gas for internal carbonization curing, increasing the mechanical strength of the cell walls, and adding phosphogypsum to optimize high temperature resistance and chemical corrosion properties, while using polycarboxylate water-reducing agent and zirconia balls to improve foam stability.
It achieves near-zero carbon emissions, excellent fire resistance, good mechanical properties and thermal insulation effects, reduces carbon dioxide emissions, and improves the compressive strength and durability of the material.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of building materials, and in particular to an insulation board for near-zero carbon emission assembled buildings and a preparation method thereof. Background Art
[0002] As the population increases, environmental resources are under increasing pressure, and building energy consumption accounts for more than 30% of total social energy consumption. It is urgent to build a resource-saving and environmentally friendly lifestyle. The Ministry of Housing and Urban-Rural Development has proposed strict energy-saving standards, and major cities in China have also taken the lead in implementing a 65% energy-saving design standard.
[0003] Foamed concrete is a concrete product with considerable strength and containing a large number of tiny closed pores formed by introducing air or nitrogen, carbon dioxide, oxygen and other gases into the concrete slurry through chemical or physical means according to application needs, and then properly cured and formed. At present, foamed concrete can be used as an insulation board because of its good thermal insulation effect, low density, light weight, thermal insulation, sound insulation and earthquake resistance.
[0004] Although organic insulation boards have good insulation effects due to their low thermal conductivity, traditional organic building insulation boards pose serious fire hazards during use. In recent years, large-scale building fires caused by the use of such organic flammable insulation boards have been common, causing hundreds of millions of dollars in significant economic losses and many casualties, seriously threatening people's lives and safety.
[0005] Therefore, developing an inorganic insulation board with near-zero carbon emissions, good safety and durability is of great significance to prefabricated buildings. Summary of the invention
[0006] In view of the problems of low carbon dioxide curing efficiency of existing inorganic insulation materials, difficulty in meeting the needs of large-size components, and poor safety and durability of organic insulation materials, a near-zero carbon emission prefabricated building insulation board and preparation method which has better mechanical properties and excellent fire resistance as well as the advantages of light weight, greenness, thermal insulation and heat insulation is provided.
[0007] The beneficial effects of the above scheme are:
[0008] 1) The present invention uses slag and magnesium slag as cementitious materials to prepare foamed concrete. Magnesium slag contains a large amount of CaO and MgO, which can increase the alkalinity of the slurry and quickly break the Al-O and Si-O bonds in the slag to form SiO 3 2- With AlO 3 3- Anion group, free Ca in the slurry 2+Further combined with the generation of hydration products with gelling properties such as CSH and CAH, it ensures that the newly mixed lightweight foam has good early strength; and the introduction of solid wastes rich in high-strength γ-C2S such as magnesium slag can also react with unreacted carbonates, and the generated carbon dioxide gas can be used for internal carbonization curing to enhance the mechanical strength and performance of the pore wall;
[0009] 2) The present invention does not add cement or cement clinker, and mainly uses industrial solid waste slag and magnesium slag as cementitious materials, which not only realizes the resource utilization of solid waste, but also has significant economic and environmental benefits; and the prepared foamed concrete has better mechanical properties and excellent fire resistance;
[0010] 3) In the present invention, sodium bicarbonate and alum are used as foaming agents to react in the slurry slurry mineral admixture A to generate carbon dioxide, thereby causing the foamed concrete to expand rapidly, and the aluminum hydroxide generated by the reaction can improve the foamed concrete;
[0011] 4) The foam stabilizer used in the present invention reduces the possibility of flocculent material generation, thereby improving the stability of foam stabilization;
[0012] 5) The addition of phosphogypsum in the present invention can not only optimize the high temperature resistance and chemical corrosion resistance of the foamed concrete, but also improve the strength and toughness of the foamed concrete. DETAILED DESCRIPTION
[0013] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0014] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0015] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.
[0016] In an embodiment of the present invention, a near-zero carbon emission prefabricated building insulation board is provided, wherein the slag powder has a median particle size D50 of 10 μm to 30 μm, and the content of the glass body is 35% to 50%; the median particle size D80 of the magnesium slag powder is 80 μm to 100 μm, and the main components are 40% to 55% of CaO, 20% to 30% of SiO 2 , 6% to 10% MgO, 2% to 5% Al 2 O 3 and 8% to 9% Fe2 O 3 ; The water reducer is a polycarboxylate water reducer, and its maximum water reduction rate is 30% to 40%; the foam stabilizer is a hydroxyethyl cellulose, polyacrylamide or EVA emulsion; the grinding medium is a zirconium oxide ball, and its size is 2.5mm to 3mm; the gypsum content in the phosphogypsum is ≥90%, and the soluble phosphorus and fluorine impurities content is ≤1%; the median particle size of the slag D50 = 10μm to 50μm, and the density is 2.21 to 2.26g / cm 3 Its main components are 65% to 68% CaO and 3% to 7% SiO 2 , 2% to 7% Al 2 O 3 And 1% to 3% Fe 2 O 3 .
[0017] Example 1
[0018] A near-zero carbon emission prefabricated building insulation board, the preparation of which includes the following steps:
[0019] 1) 140 parts of slag powder, 40 parts of magnesium slag powder, 80 parts of water, 1 part of water reducer and 300 parts of grinding media were placed in a ball mill and ground for 90 minutes to obtain a slurry mineral admixture A with a median particle size D50 of 4 μm;
[0020] 2) 10 parts of sodium bicarbonate, 4 parts of alum, 5 parts of phosphogypsum and 10 parts of carbide slag were placed in a mortar mixer and mixed for 4 minutes to obtain dry powder B;
[0021] 3) Take slurry mineral admixture A, dry powder B and 2 parts of foam stabilizer and mix them in a mortar mixer for 2 minutes;
[0022] 4) After pouring the evenly stirred foam concrete slurry into the mold, immediately put it into the curing box for curing. The curing temperature is 40° C. and the humidity is maintained above 85%. After curing for 6 hours, the mold is removed and cut to obtain a near-zero carbon emission prefabricated building insulation board.
[0023] Example 2
[0024] A near-zero carbon emission prefabricated building insulation board, the preparation of which includes the following steps:
[0025] 1) 150 parts of slag powder, 50 parts of magnesium slag powder, 90 parts of water, 2 parts of water reducer and 350 parts of grinding media were placed in a ball mill and ground for 60 minutes to obtain a slurry mineral admixture A with a median particle size D50 of 5 μm;
[0026] 2) 9 parts of sodium bicarbonate, 5 parts of alum, 7 parts of phosphogypsum and 12.5 parts of carbide slag were placed in a mortar mixer and mixed for 3 minutes to obtain dry powder B;
[0027] 3) Take slurry mineral admixture A, dry powder B and 2 parts of foam stabilizer and mix them in a mortar mixer for 2 minutes;
[0028] 4) After pouring the evenly stirred foam concrete slurry into the mold, it is immediately placed in a curing box for curing. The curing temperature is 50° C. and the humidity is maintained above 85%. After curing for 7 hours, the mold is removed and cut to obtain a near-zero carbon emission prefabricated building insulation board.
[0029] Example 3
[0030] 1) 160 parts of slag powder, 60 parts of magnesium slag powder, 100 parts of water, 2 parts of water reducer and 400 parts of grinding medium were placed in a ball mill and ground for 120 minutes to obtain a slurry mineral admixture A with a median particle size D50 of 3 μm;
[0031] 2) 8 parts of sodium bicarbonate, 5 parts of alum, 10 parts of phosphogypsum and 15 parts of carbide slag were placed in a mortar mixer and mixed for 5 minutes to obtain dry powder B;
[0032] 3) Take slurry mineral admixture A, dry powder B and 2 parts of foam stabilizer and mix them in a mortar mixer for 3 minutes;
[0033] 4) After pouring the evenly mixed foam concrete slurry into the mold, immediately put it into the curing box for curing. The curing temperature is 60° C. and the humidity is maintained above 85%. After curing for 8 hours, the mold is removed and cut to obtain a near-zero carbon emission prefabricated building insulation board.
[0034] Comparative Example 1
[0035] A 400 bulk density grade foam concrete board, the preparation method of which is as follows:
[0036] 1) Add 100 parts of Portland cement, 10 parts of fly ash and 0.05 parts of foam stabilizer into a mixer and stir at a rate of 125 r / min for 1 min;
[0037] 2) Weigh 55 parts of water and 0.2 parts of water reducer into a mixer and stir at a rate of 125±5r / min for 1 minute;
[0038] 3) Weigh 2.5 parts of a foaming agent and add it into the above mixer, stir at a rate of 62±5 r / min for 30 seconds, pour, and cure in an environment of 20±2° C. and humidity ≥95% to obtain 400 bulk density grade foamed concrete.
[0039] Comparative Example 2
[0040] A 600 bulk density grade foam concrete board, the preparation method of which is as follows:
[0041] 1) Add 100 parts of Portland cement, 30 parts of fly ash and 0.04 parts of foam stabilizer into a mixer and stir at a rate of 125 r / min for 1 min;
[0042] 2) Weigh 55 parts of water and 0.2 parts of water reducer into a mixer and stir at a rate of 125±5r / min for 1 minute;
[0043] 3) Weigh 2.2 parts of foaming agent and add it into the above mixer, stir at a rate of 62±5r / min for 30s, pour, and cure in an environment of 20±2°C and humidity ≥95% to obtain 600 bulk density grade foamed concrete.
[0044] The comparative examples and embodiments were subjected to performance tests, wherein the dry density of the insulation board was tested according to the Technical Specification for Lightweight Aggregate Concrete (JGJ512002), and the compressive strength of the insulation board was tested according to the standard test method for mechanical properties of ordinary concrete. The carbon dioxide emissions are calculated based on the cement consumption and the energy consumption of mechanical grinding and mixing, calculated as 860kg per ton of cement; the grinder is calculated based on the conventional 5t / h capacity of 75kw, calculated as an average of 0.785kg / kw·h; the maintenance energy consumption is calculated based on the data collected from the production line of 16.6kw·h / cubic meter. The amount of carbon dioxide consumed is mainly the amount of carbon consumed in the sodium bicarbonate. The test results are shown in the following table:
[0045]
[0046] As can be seen from the above table, the thermal conductivity of the foamed concrete insulation board prepared in Examples 1 to 3 of the present invention reaches below 0.18 W / m·K, the compressive strength reaches above 2.2 MPa, and the dry density reaches 483 Kg / m 3 The above has good thermal insulation, heat insulation and compression resistance.
[0047] In addition, the thermal conductivity of the foam concrete insulation board prepared in Examples 1 to 3 of the present invention is increased compared with that of Comparative Examples 1 and 2, while the thermal insulation performance is reduced, and the compressive strength, acid resistance, and alkali resistance are all reduced to varying degrees. This may be because solid wastes such as magnesium slag are rich in high-strength γ-C2S, which can react with unreacted carbonates. At the same time, the carbon dioxide gas generated by the reaction has a lower thermal conductivity, which enhances the thermal insulation effect of the material.
[0048] The above description is only a preferred embodiment of the present invention, and does not limit the implementation mode and protection scope of the present invention. For those skilled in the art, it should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of the specification of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a near-zero carbon emission prefabricated building insulation board, characterized in that: The steps include: 1) 140-160 parts of slag powder, 40-60 parts of magnesium slag powder, 80-100 parts of water, 1-2 parts of water reducer and 300-400 parts of grinding media are placed in a ball mill and ground for 60-120 min to obtain a slurry mineral admixture A with a median particle size D50 = 3 μm-5 μm; 2) Take 8-10 parts of sodium bicarbonate, 4-5 parts of alum, 5-10 parts of phosphogypsum and 10-15 parts of carbide slag and mix them in a mortar mixer for 3-5 minutes to obtain dry powder B; 3) Take slurry mineral admixture A, dry powder B and 2-4 parts of foam stabilizer and mix them in a mortar mixer for 2-3 minutes; 4) After pouring the evenly mixed foam concrete slurry into the mold, immediately put it into the curing box for curing. The curing temperature is 40℃~60℃, and the humidity is maintained above 85%. After curing for 6~8h, the mold is removed and cut to obtain a near-zero carbon emission prefabricated building insulation board.
2. The preparation method according to claim 1, characterized in that: The median particle size of the slag powder is D50=10 μm~30 μm; the content of glass is 35%~50%.
3. The preparation method according to claim 1, characterized in that: The median particle size of the magnesium slag powder is D80=80 μm~100 μm, and its main components are 40%~55% CaO, 20%~30% SiO2, 6%~10% MgO, 2%~5% Al2O3 and 8%~9% Fe2O3.
4. The preparation method according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid water reducing agent, and its maximum water reducing rate is 30% to 40%.
5. The preparation method according to claim 1, characterized in that: The foam stabilizer is one of hydroxyethyl cellulose, polyacrylamide or EVA emulsion.
6. The preparation method according to claim 1, characterized in that: The grinding medium is a zirconia ball with a size of 2.5 mm to 3 mm.
7. The preparation method according to claim 1, characterized in that: The gypsum content in the phosphogypsum is ≥90%, and the soluble phosphorus and fluorine impurity content is ≤1%.
8. The preparation method according to claim 1, characterized in that: The median particle size of the carbide slag is D50=10 μm~50 μm, and the density is 2.21~2.26 g / cm 3 Its main components are 65%~68% CaO, 3%~7% SiO2, 2%~7% Al2O3 and 1%~3% Fe2O3.
9. A near-zero carbon emission prefabricated building insulation board, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 8.