Semiconductor devices and methods for fabricating semiconductor devices
By setting p-type doped layers with different thicknesses and doping concentrations in GaN devices, the edge electric field and hole injection are adjusted, solving the dynamic resistance degradation problem, reducing on-resistance, and improving device performance and reliability.
Patent Information
- Application Number
- CN202310287863.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-16
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-03-16
AI Technical Summary
GaN devices experience increased on-resistance due to dynamic resistance degradation during switching, affecting device performance and reliability. This is particularly evident in high-frequency converter applications where power loss is significant, and existing optimization techniques only exacerbate the on-resistance increase.
A p-type doped layer is set in the injection region of the semiconductor stack. The p-type doped layers with different doping concentrations and/or thicknesses form a PN junction with the semiconductor stack. Holes are injected to adjust the edge electric field, reduce the hot carrier effect, and suppress electric field degradation.
By adjusting the edge electric field and hole injection capability, the on-resistance is reduced, the reliability and dynamic behavior of the device are improved, the damage of hot carriers to the device is reduced, and the dynamic resistance and on-resistance performance are optimized.
Smart Images

Figure CN116417514B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor devices, and more specifically, to a method for fabricating semiconductor devices. Background Technology
[0002] Currently, the main challenges facing the use of GaN devices include improving device performance and overcoming existing defects. For example, one problem encountered during device operation is dynamic resistance degradation, also known as current collapse. This is a common reliability issue in planar GaN devices, referring to the phenomenon where, in the switching state, the channel carriers are partially depleted due to surface defects and epitaxial layer (EPI) defects, leading to increased on-resistance and conduction losses. In other words, after a GaN device has been subjected to high-voltage bias for a period of time and then switched on, the actual on-voltage will be higher than the ideal value.
[0003] Studies have shown that as the on-time of a device increases, its on-resistance gradually decreases, eventually recovering to the ideal on-resistance value (static value) after a sufficiently long period. This recovery time is not yet precisely defined, but it ranges from 0.1 to 1000 seconds. However, in practical power electronic applications, switching devices need to continuously switch between on and off states at high speeds, with switching frequencies exceeding 100 kHz. This means that the on-time of the device within each duty cycle is very short, insufficient for the on-resistance to recover to its static value. Therefore, in high-frequency converter applications, the increase in on-resistance caused by dynamic resistance degradation will be significant, greatly increasing power loss, reducing device efficiency, and severely limiting the widespread application of GaN power devices.
[0004] The presence of these charge carriers in the device can trigger numerous physical damage phenomena, which can drastically alter the device's characteristics and ultimately lead to circuit failure. While existing technologies offer solutions to optimize the device's dynamic resistance, these often result in increased on-resistance, which also affects device performance. Therefore, a novel HEMT structure is needed to prevent hot carrier effects, thereby improving device performance and reliability. Summary of the Invention
[0005] The objectives of this invention include, for example, providing a semiconductor device and a method for fabricating a semiconductor device, which can optimize the electric field at the drain edge, improve the hot carrier effect, optimize the dynamic resistance and reliability of the semiconductor device, and reduce the on-resistance.
[0006] The embodiments of the present invention can be implemented as follows:
[0007] In a first aspect, the present invention provides a semiconductor device, comprising:
[0008] Substrate;
[0009] Semiconductor stacks disposed on a substrate;
[0010] and the source, gate, and drain electrodes disposed on the semiconductor stack;
[0011] The drain electrode includes a drain metal layer and a p-type doped layer. The p-type doped layer is disposed in the implantation region of the semiconductor stack and is used to implant holes into the implantation region of the semiconductor stack. The doping concentration and / or thickness of the p-type doped layer are different at different positions in the implantation region to adjust the hole implantation capability at different positions in the implantation region and to adjust the edge electric field of the implantation region. The drain metal layer at least partially covers the p-type doped layer and is in ohmic contact with the semiconductor stack.
[0012] In an optional embodiment, the implantation region has a middle region and an edge region along the width direction, and the thickness of the p-type doped layer corresponding to the middle region is different from the thickness of the p-type doped layer corresponding to the edge region.
[0013] In an optional implementation, the thickness of the p-type doped layer corresponding to the middle region is less than the thickness of the p-type doped layer corresponding to the edge region.
[0014] In an optional implementation, the doping concentration of the p-type doped layer corresponding to the intermediate region is less than or equal to the thickness of the p-type doped layer corresponding to the edge region.
[0015] In an optional embodiment, the p-type doped layer includes a first doped layer and a second doped layer, wherein the first doped layer is disposed on the semiconductor stack, and the second doped layer is disposed on the first doped layer and disposed on both sides of the first doped layer.
[0016] In an optional implementation, the doping concentration of the first doped layer is different from that of the second doped layer.
[0017] In an optional embodiment, the implantation region has a middle region and an edge region along the width direction, and the thickness of the p-type doped layer corresponding to the middle region is greater than the thickness of the p-type doped layer corresponding to the edge region.
[0018] In an optional implementation, the doping concentration of the p-type doped layer corresponding to the intermediate region is less than the doping concentration of the p-type doped layer corresponding to the edge region.
[0019] In an optional embodiment, the implantation region has a middle region and an edge region along the width direction. The thickness of the p-type doped layer corresponding to the middle region is equal to the thickness of the p-type doped layer corresponding to the edge region, and the doping concentration of the p-type doped layer corresponding to the middle region is different from the doping concentration of the p-type doped layer corresponding to the edge region.
[0020] In an optional embodiment, the p-type doped layer includes a plurality of p-type doped islands, which are uniformly spaced apart in the implantation region. The drain metal layer is deposited in the region between two adjacent p-type doped islands and partially covers the p-type doped islands. Each p-type doped island extends to both ends along the width direction of the implantation region and is exposed outside the drain metal layer to block the drain metal layer on the p-type doped island from the semiconductor stack.
[0021] In an optional embodiment, the drain metal layer between two adjacent p-type doped islands extends to both sides to form a field plate portion, which is spaced apart from the semiconductor stack and is used to adjust the edge electric field of the implantation region.
[0022] In an optional embodiment, the semiconductor device further includes a dielectric layer covering the semiconductor stack, wherein the source, the gate, and the drain metal are all exposed in the dielectric layer.
[0023] Secondly, the present invention provides a method for fabricating a semiconductor device, applicable to the semiconductor device described in any of the foregoing embodiments, the method comprising:
[0024] Provide a substrate;
[0025] A semiconductor stack is formed on the substrate;
[0026] A gate and a p-type doped layer are formed on the semiconductor stack;
[0027] Source and drain metal layers are formed on the semiconductor stack;
[0028] The p-type doped layer is disposed in the implantation region of the semiconductor stack and is used to inject holes into the implantation region of the semiconductor stack. The doping concentration and / or thickness of the p-type doped layer are different at different positions in the implantation region to adjust the hole injection capability at different positions in the implantation region and to adjust the edge electric field of the implantation region. The drain metal layer at least partially covers the p-type doped layer and is in ohmic contact with the semiconductor stack.
[0029] In an optional embodiment, the step of forming a gate and a p-type doped layer on the semiconductor stack includes:
[0030] A gate is formed on the semiconductor stack;
[0031] A p-type doped layer is deposited in the implantation region of the semiconductor stack;
[0032] The middle part of the p-type doped layer is thinned.
[0033] In an optional embodiment, the step of forming a gate and a p-type doped layer on the semiconductor stack includes:
[0034] A gate is formed on the semiconductor stack;
[0035] A first doped layer is deposited in the implantation region of the semiconductor stack;
[0036] A second doped layer is deposited at both edges of the first doped layer.
[0037] In an optional embodiment, the step of forming a gate and a p-type doped layer on the semiconductor stack includes:
[0038] A gate is formed on the semiconductor stack;
[0039] A p-type doped layer is deposited in the implantation region of the semiconductor stack;
[0040] The p-type doped layer is etched to divide it into multiple p-type doped islands.
[0041] The beneficial effects of the embodiments of the present invention include, for example:
[0042] The semiconductor device and its fabrication method provided in this invention involve depositing a p-type doped layer in the implantation region of a semiconductor stack, followed by a drain metal layer on the p-type doped layer and the semiconductor stack. The drain metal layer at least partially covers the p-type doped layer and is in ohmic contact with the semiconductor stack. The p-type doped layer is used to inject holes into the implantation region, and the doping concentration and / or thickness of the p-type doped layer varies at different locations within the implantation region. This allows for adjustment of the hole injection capability at different locations within the implantation region and regulation of the edge electric field of the implantation region. Compared to existing technologies, this invention, by setting a p-type doped layer, can form a PN junction with the semiconductor stack to generate holes, i.e., inject holes into the semiconductor stack. These holes can capture electrons that accidentally penetrate certain regions of the semiconductor due to the high electric field bombardment caused by the high voltage applied to the drain, thereby reducing the number of hot carrier electrons and thus reducing their damage to the device. This suppresses the electric field at the drain edge, reduces resistance degradation, and improves the reliability and dynamic behavior of the device. Furthermore, due to the different doping concentrations and / or thicknesses in different regions, their hole injection capabilities vary, preventing excessive depletion of the two-dimensional electron gas in some regions. This reduces the on-resistance and achieves a relatively lower on-resistance, resulting in superior dynamic resistance and on-resistance performance. Attached Figure Description
[0043] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0044] Figure 1 This is a schematic diagram of the structure of a semiconductor device in the prior art;
[0045] Figure 2 A schematic diagram of the structure of a semiconductor device provided in the first embodiment of the present invention from a first perspective;
[0046] Figure 3 A schematic diagram of the semiconductor device provided in the first embodiment of the present invention from a second perspective;
[0047] Figure 4 This is a schematic diagram of the semiconductor device provided in the first embodiment of the present invention from a third-view perspective;
[0048] Figures 5 to 6 This is a partial process flow diagram of the method for fabricating a semiconductor device according to the first embodiment of the present invention;
[0049] Figure 7This is a schematic diagram of the structure of a semiconductor device provided in the second embodiment of the present invention;
[0050] Figures 8 to 10 This is a partial process flow diagram of the method for fabricating a semiconductor device according to the second embodiment of the present invention;
[0051] Figure 11 This is a schematic diagram of the structure of a semiconductor device provided in the third embodiment of the present invention;
[0052] Figure 12 This is a schematic diagram of the structure of a semiconductor device provided in the fifth embodiment of the present invention from a first perspective;
[0053] Figure 13 for Figure 12 Cross-sectional view at point AA;
[0054] Figure 14 for Figure 12 Sectional view at point BB;
[0055] Figure 15 This is a schematic diagram of the semiconductor device provided in the fifth embodiment of the present invention from a second perspective.
[0056] Figures 16 to 18 This is a partial process flow diagram of the semiconductor device fabrication method provided in the fifth embodiment of the present invention.
[0057] Icons: 100 - Semiconductor device; 110 - Substrate; 120 - Semiconductor stack; 121 - Buffer layer; 123 - Channel layer; 125 - Barrier layer; 130 - Source; 140 - Gate; 150 - Drain; 151 - Drain metal layer; 153 - p-type doped layer; 155 - First doped layer; 157 - Second doped layer; 158 - Field plate; 159 - p-type doped island; 160 - Dielectric layer. Detailed Implementation
[0058] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.
[0059] Therefore, the following detailed description of the embodiments of the invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the invention without inventive effort are within the scope of protection of the invention.
[0060] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.
[0061] In the description of this invention, it should be noted that if terms such as "upper," "lower," "inner," or "outer" are used to indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship in which the product of this invention is usually placed, they are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention.
[0062] Furthermore, the terms "first" and "second" are used only to distinguish descriptions and should not be interpreted as indicating or implying relative importance.
[0063] Currently, first-generation semiconductors represented by Si and second-generation semiconductor materials represented by GaAs have limitations. Third-generation wide-bandgap semiconductor materials (GaN, SiC) have seen rapid development due to their superior performance. GaN, as one of the core materials of third-generation semiconductors, is unique compared to Si, GaAs, and SiC in its polarization effect. Utilizing this unique property, AlGaN / GaN high electron mobility transistors (AlGaN / GaN HEMTs) have been developed. AlGaN / GaN HEMTs are GaN-based microelectronic devices fabricated based on AlGaN / GaN heterojunction materials. The AlGaN / GaN heterojunction forms a high-density two-dimensional electron gas (2DEG) at the heterojunction interface through spontaneous polarization and piezoelectric polarization effects. This 2DEG has a high mobility, leading to an increase in carrier concentration at the heterojunction interface, thus meeting the requirements of high-power / high-frequency devices.
[0064] Currently, the main challenges facing the use of GaN devices include improving device performance and overcoming existing defects. For example, one problem encountered during device operation is dynamic resistance degradation, also known as current collapse, a common reliability issue in planar GaN devices. This refers to the phenomenon where, in the switching state, GaN devices experience partial depletion of channel carriers due to surface defects and epitaxial layer (EPI) defects, leading to increased on-resistance and conduction losses. In other words, after a GaN device has been subjected to high-voltage bias for a period and then switched to the on-state, the actual on-voltage will be higher than the ideal value. Research shows that as the device's on-time increases, the on-resistance gradually decreases, eventually recovering to the ideal on-resistance value (static value) after a sufficiently long period. This recovery time is not yet precisely defined, but it ranges from 0.1 to 1000 seconds. However, in practical power electronics applications, switching devices need to continuously switch between on and off states at high speeds, with switching frequencies exceeding hundreds of kHz. This means that the device is on for a very short time in each duty cycle, insufficient for the on-resistance to return to its static value. Therefore, in high-frequency converter applications, the increase in on-resistance caused by dynamic resistance degradation will be very significant, which will greatly increase the device's power loss, reduce its operating efficiency, and severely restrict the widespread application of GaN power devices.
[0065] The inventors' research revealed two main mechanisms underlying the aforementioned problems. One is the formation of a virtual gate. When the device operates in a high-voltage blocking state, the surface electric field between the gate and drain accelerates electrons in the material, exciting them and causing them to be trapped by traps on the AlGaN barrier layer surface. These surface traps primarily originate from material defects, etching, or implantation damage. Consequently, the trapped electrons accumulate negative charges in the region between the gate and drain. These surface negative charges act as a negatively biased gate (i.e., a virtual gate), lowering the surface potential and partially depleting the underlying two-dimensional electron gas, thus increasing the on-resistance. The other mechanism is the channel hot electron injection effect. At the moment the device is turned on, electrons in the channel are accelerated into high-energy hot electrons by a strong electric field. These hot electrons have sufficient energy to escape from the channel and inject into surface traps in the barrier layer, heterojunction interface traps, or deeper buffer layer traps. These traps mainly originate from crystal defects and compensating doping in the material itself. When the device is turned on, the trapped electrons are slowly released from the traps, gradually restoring the two-dimensional electron gas. If the on-time is long enough, the on-resistance will gradually recover to its initial value. The recovery speed is determined by the time constant, which is related to many factors such as the trap energy level and temperature.
[0066] The presence of these charge carriers in the device can trigger numerous physical damage phenomena that drastically alter the device's characteristics and ultimately lead to circuit failure. Therefore, a novel HEMT structure is needed to prevent hot carrier effects, thereby improving device performance and reliability.
[0067] For enhancement-mode devices, when the potential at the drain edge changes drastically, the electric field strength at the drain edge increases with the drain voltage. Therefore, the high electric field in this region can gain energy through bombardment of ionized electrons, accidentally penetrating certain areas of the semiconductor, leading to permanent degradation and serious reliability issues. Therefore, existing technologies have developed schemes to optimize the dynamic resistance of the device, such as... Figure 1 The structure disclosed herein, which introduces an additional semiconductor layer into the drain metal, can form a PN junction with the barrier layer to generate holes, thereby improving the reliability and dynamic behavior of the device. However, this technique typically involves adding an entire semiconductor layer along the gate width direction in the drain. The hole injection capability of the semiconductor layer is uniform and optimal, resulting in greater depletion of the two-dimensional electron gas and a problem of relatively high on-resistance.
[0068] To address the aforementioned problems, this invention provides a novel semiconductor device that can adjust the edge electric field on both sides of the drain while injecting holes, and prevents the two-dimensional electron gas in the barrier layer from being excessively depleted, thus preventing an excessive increase in on-resistance and relatively reducing on-resistance, thereby solving the problem of excessively high on-resistance. It should be noted that, unless otherwise specified, the features in the embodiments of this invention can be combined with each other.
[0069] First Embodiment
[0070] Please see Figures 2 to 4 This invention provides a semiconductor device 100 that can reduce the number of electrons in the form of hot carriers, thereby reducing their damage to the device and suppressing the electric field at the edge of the drain 150. This reduces resistance degradation and improves the device's reliability and dynamic behavior. Furthermore, it prevents the on-resistance from increasing too much, achieving a relatively lower on-resistance and thus achieving superior dynamic resistance and on-resistance performance.
[0071] The semiconductor device 100 provided in this embodiment includes a substrate 110, a semiconductor stack 120, a source 130, a gate 140, and a drain 150. The semiconductor stack 120 is disposed on the substrate 110, and the source 130, gate 140, and drain 150 are disposed on the semiconductor stack 120. The drain 150 includes a drain metal layer 151 and a p-type doped layer 153. The p-type doped layer 153 is disposed in the implantation region of the semiconductor stack 120 and is used to implant holes into the implantation region of the semiconductor stack 120. The doping concentration and / or thickness of the p-type doped layer 153 are different at different positions in the implantation region to adjust the hole implantation capability at different positions in the implantation region and to adjust the edge electric field of the implantation region. The drain metal layer 151 at least partially covers the p-type doped layer 153 and is in ohmic contact with the semiconductor stack 120.
[0072] The semiconductor stack 120 includes a buffer layer 121, a channel layer 123, and a barrier layer 125. The buffer layer 121 is disposed on the substrate 110, the channel layer 123 is disposed on the buffer layer 121, and the barrier layer 125 is disposed on the channel layer 123. Its specific interlayer structure is consistent with that of a conventional enhancement-mode transistor, and will not be described in detail here.
[0073] In this embodiment, the material of the substrate 110 can be, but is not limited to, group III-V elements or combinations thereof. Examples include Si, SiGe, SiC, GaAs, p-doped Si, n-doped Si, sapphire, etc. The material of the buffer layer 121 includes, but is not limited to, nitrides or combinations of group III-V elements. For example, the buffer layer 121 can be AlN, InN, GaN, AlGaN, AlInGaN, etc. The buffer layer 121 can reduce lattice mismatch and thermal mismatch between the substrate 110 and the layers formed on the buffer layer 121, repairing defects such as imperfections. The channel layer 123 can be GaN, and the barrier layer 125 can be ALGAN. A triangular potential well is generated between the channel layer 123 and the barrier layer 125, where electrons accumulate and a two-dimensional electron gas (2DEG) is generated at the interface. The gate 140 material can be a p-type doped group III-V compound / nitride semiconductor layer; the source 130 material and the drain metal layer 151 material can be aluminum or gold. The p-type doped layer 153 can be a p-type doped III-V compound / nitride semiconductor layer, and can be a material similar to or not exactly the same as the gate 140.
[0074] In this embodiment, the semiconductor device 100 may further include a dielectric layer 160, which covers the semiconductor stack 120, and the source 130, gate 140, and drain 150 metals are all exposed in the dielectric layer 160. Specifically, the dielectric layer 160 covers the barrier layer 125, enclosing the periphery of the source 130, gate 140, and drain 150 metals. The dielectric layer 160 may be silicon dioxide or silicon nitride material.
[0075] In this embodiment, the p-type doped layer 153 is used to inject holes into the injection region, and the doping concentration and / or thickness of the p-type doped layer 153 are different at different locations in the injection region, i.e., there are three cases: 1. The doping concentration of the p-type doped layer 153 is different at different locations in the injection region; 2. The thickness of the p-type doped layer 153 is different at different locations in the injection region; 3. The doping concentration and thickness of the p-type doped layer 153 are both different at different locations in the injection region. This setting can adjust the hole injection capability at different locations in the injection region and adjust the edge electric field of the injection region. By setting a p-type doped layer 153, holes can be generated by forming a PN junction with the semiconductor stack 120, i.e., holes are injected into the semiconductor stack 120. These holes can capture electrons that accidentally penetrate certain regions of the semiconductor due to the high electric field bombardment caused by the high voltage applied to the drain 150, thereby reducing the number of hot carrier electrons and thus reducing their damage to the device. This suppresses the electric field at the edge of the drain 150, reduces resistance degradation, and improves device reliability and dynamic behavior. Furthermore, due to the different doping concentrations and / or thicknesses in different regions, their hole injection capabilities vary, preventing excessive depletion of the two-dimensional electron gas in some regions. This prevents a significant increase in on-resistance, achieving a relatively lower on-resistance and resulting in superior dynamic resistance and on-resistance performance.
[0076] In this embodiment, the thickness of the p-type doped layer 153 varies at different locations in the implantation region. Specifically, the implantation region has a middle region and an edge region along its width direction. The thickness of the p-type doped layer 153 corresponding to the middle region is different from that corresponding to the edge region, thereby providing different hole injection capabilities and ensuring that the two-dimensional electron gas in the implantation region corresponding to the thinner p-type doped layer 153 is not depleted as much, thus relatively reducing the on-resistance.
[0077] It should be noted that the injection area here is along the width direction, that is, the gate width direction.
[0078] Preferably, in this embodiment, the thickness of the p-type doped layer 153 corresponding to the middle region is less than the thickness of the p-type doped layer 153 corresponding to the edge region. The p-type doped layer 153 has a structure that is thicker at both ends and thinner in the middle, making its cross-sectional shape concave. This structure, which is thinner in the middle and thicker at both ends, can adjust the edge electric field on both sides of the drain 150 while injecting holes, and at the same time, it can prevent the two-dimensional electron gas in the middle region of the drain 150 from being depleted too much, so that the on-resistance does not increase so much.
[0079] It should be noted that, in this embodiment, the drain metal layer 151 is wrapped around the periphery along the shape of the p-type doped layer 153 during fabrication, thereby completely covering the p-type doped layer 153. The drain metal layer 151 located on both sides of the p-type doped layer 153 is in direct contact with the barrier layer 125, thereby ensuring ohmic contact between the drain metal layer 151 and the barrier layer 125. Furthermore, the shape of the drain metal layer 151 is not specifically limited here.
[0080] This embodiment also provides a method for fabricating a semiconductor device 100, which is used to fabricate the aforementioned semiconductor device 100. The fabrication method includes:
[0081] S1: Provide a substrate 110.
[0082] Specifically, the material of the substrate 110 may include, but is not limited to, group III-V elements or combinations thereof. For example, Si, SiGe, SiC, GaAs, p-doped Si, n-doped Si, sapphire, etc.
[0083] S2: A semiconductor stack 120 is formed on the substrate 110.
[0084] Specifically, a buffer layer 121, a channel layer 123, and a barrier layer 125 are sequentially formed on the substrate 110. The material of the buffer layer 121 includes, but is not limited to, nitrides or combinations of group III-V elements. For example, the buffer layer 121 can be AlN, InN, GaN, AlGaN, AlInGaN, etc. The buffer layer 121 can reduce lattice mismatch and thermal mismatch between the substrate 110 and the layers formed on the buffer layer 121, and repair defects such as defects caused by these mismatches. The channel layer 123 can be GaN, and the barrier layer 125 can be ALGAN. A triangular potential well is generated between the channel layer 123 and the barrier layer 125, where electrons accumulate and a two-dimensional electron gas (2DEG) is generated at the interface.
[0085] S3: A gate 140 and a p-type doped layer 153 are formed on the semiconductor stack 120.
[0086] Specifically, please see Figure 5 and Figure 6A p-type doped layer 153 is disposed in the implantation region of the semiconductor stack 120 to implant holes into the implantation region of the semiconductor stack 120, and the thickness of the p-type doped layer 153 varies at different locations in the implantation region. Preferably, a gate 140 can be formed on the semiconductor stack 120, and then the p-type doped layer 153 can be deposited in the implantation region of the semiconductor stack 120. Then, the middle part of the p-type doped layer 153 is thinned to form a p-type doped layer 153 that is thin in the middle and thick at both sides, thereby adjusting the hole implantation capability at different locations in the implantation region. In actual fabrication, the gate 140 material and the p-type doped layer 153 can be fabricated first on the semiconductor stack 120, and then the unnecessary middle part of the p-type doped layer 153 below the drain 150 region can be thinned. Specifically, the middle thinning can be achieved through an etching process to complete the fabrication of the p-type doped layer 153.
[0087] It should be noted that when the material of the p-type doped layer 153 is the same as that of the gate 140, the gate 140 and the p-type doped layer 153 can be formed together.
[0088] S4: A source 130 and a drain metal layer 151 are formed on the semiconductor stack 120;
[0089] For details, please continue to see Figure 3 After completing step S3, source and drain metals can be deposited, i.e., source 130 and drain metal layer 151 are deposited. The drain metal layer 151 at least partially covers the p-type doped layer 153 and makes ohmic contact with the semiconductor stack 120. Specifically, the drain metal layer 151 wraps around the periphery along the shape of the p-type doped layer 153, and the peripheral drain metal layer 151 makes ohmic contact with the semiconductor stack 120.
[0090] In summary, this embodiment provides a semiconductor device 100 and its fabrication method. By providing a p-type doped layer 153 in the implantation region of the semiconductor stack 120, and then providing a drain metal layer 151 on the p-type doped layer 153 and the semiconductor stack 120, the drain metal layer 151 at least partially covers the p-type doped layer 153 and is in ohmic contact with the semiconductor stack 120. The p-type doped layer 153 is used to implant holes into the implantation region, and the thickness of the p-type doped layer 153 is different at different positions in the implantation region, thereby adjusting the hole implantation capability at different positions in the implantation region and adjusting the edge electric field of the implantation region. Compared to existing technologies, this embodiment, by setting a p-type doped layer 153, can form a PN junction with the semiconductor stack 120 to generate holes, i.e., inject holes into the semiconductor stack 120. These holes can capture electrons that accidentally penetrate certain regions of the semiconductor due to the high electric field bombardment generated by the high voltage applied to the drain 150, thereby reducing the number of hot carrier electrons and thus reducing their damage to the device. This suppresses the electric field at the edge of the drain 150, reducing resistance degradation and improving device reliability and dynamic behavior. Furthermore, because different regions have different thicknesses, their hole injection capabilities vary, preventing excessive depletion of the two-dimensional electron gas in some regions, thus preventing a significant increase in on-resistance and achieving a relatively lower on-resistance, resulting in superior dynamic resistance and on-resistance performance.
[0091] Second Embodiment
[0092] This embodiment provides a semiconductor device 100, whose basic structure, principle, and technical effects are the same as those of the first embodiment. For the sake of brevity, any parts not mentioned in this embodiment can be referred to the corresponding content in the first embodiment.
[0093] See Figure 7 In this embodiment, the thickness of the p-type doped layer 153 in the middle region is less than the thickness of the p-type doped layer 153 in the edge region. The p-type doped layer 153 includes a first doped layer 155 and a second doped layer 157. The first doped layer 155 is disposed on the semiconductor stack 120, and the second doped layer 157 is disposed on the first doped layer 155 and at both sides of the first doped layer 155. Specifically, the first doped layer 155 and the second doped layer 157 can be made of the same material, and the second doped layer 157 covers both sides of the first doped layer 155, thus leaving the middle of the first doped layer 155 uncovered, resulting in a structure where the p-type doped layer 153 is thin in the middle and thick at the edges.
[0094] In this embodiment, the doping concentration of the first doped layer 155 is different from that of the second doped layer 157. Of course, in other preferred embodiments of the present invention, the doping concentrations of the first doped layer 155 and the second doped layer 157 may be the same, and the materials of the first doped layer 155 and the second doped layer 157 may also be different, which is not specifically limited here.
[0095] This embodiment also provides a method for fabricating a semiconductor device 100, the basic steps and principles of which are the same as those in the first embodiment, and the resulting technical effects are the same. For the sake of brevity, any parts not mentioned in this embodiment can be referred to the corresponding content in the first embodiment. Compared with the first embodiment, the difference in the fabrication method provided in this embodiment lies in the fabrication of the p-type doped layer 153.
[0096] See also Figures 8 to 10 In this embodiment, step S3, which forms a gate 140 and a p-type doped layer 153 on the semiconductor stack 120, includes: forming a gate 140 on the semiconductor stack 120, then depositing a first doped layer 155 in the implantation region of the semiconductor stack 120; and then depositing a second doped layer 157 at both edges of the first doped layer 155. Specifically, in actual fabrication, a thin layer of the required gate 140 material and a first doped layer 155 can be formed on the semiconductor stack 120 first. Then, chemical vapor deposition is performed to grow another layer of semiconductor material, i.e., to form a second doped layer 157. Then, the middle position of the second doped layer 157 is thinned by etching so that the second doped layer 157 only covers the two edge regions of the first doped layer 155. Then, source and drain metals are deposited, i.e., source 130 and drain metal layers 151 are deposited. The drain metal layer 151 wraps around the periphery along the shape of the p-type doped layer 153, and the outer drain metal 150 contacts the p-type doped layer 153 to form an ohmic contact.
[0097] Specifically, the double-layer deposition method used in this embodiment allows for precise control of the material thickness in the thinner region of the p-type doped layer 153. That is, when etching the second doped layer 157, the first doped layer 155 can be used as an etching stop layer, ensuring that the thickness of the thinner region of the p-type doped layer 153 is comparable to the thickness of the first doped layer 155. Furthermore, this approach allows for different doping concentrations in the upper and lower first doped layers 155 and the second doped layer 157, resulting in different effects.
[0098] Third Embodiment
[0099] See Figure 11 This embodiment provides a semiconductor device 100, whose basic structure, principle and technical effects are the same as those of the first embodiment. For the sake of brevity, any parts not mentioned in this embodiment can be referred to the corresponding content in the first embodiment.
[0100] In this embodiment, the implantation region has a middle region and an edge region along its width direction. The thickness of the p-type doped layer 153 corresponding to the middle region is greater than the thickness of the p-type doped layer 153 corresponding to the edge region. Specifically, the p-type doped layer 153 corresponding to the middle region is thicker, making the overall p-type doped layer 153 exhibit a "convex" shaped structure, thereby making the hole implantation capabilities of the middle region and the edge region different.
[0101] In this embodiment, the doping concentration of the p-type doped layer 153 corresponding to the middle region is less than the doping concentration of the p-type doped layer 153 corresponding to the edge region.
[0102] In other preferred embodiments of the present invention, the p-type doped layer 153 may also be formed by a combination of concave and convex structures.
[0103] Fourth embodiment
[0104] This embodiment provides a semiconductor device 100, whose basic structure, principle, and technical effects are the same as those of the first embodiment. For the sake of brevity, any parts not mentioned in this embodiment can be referred to the corresponding content in the first embodiment.
[0105] In this embodiment, the implantation region has a middle region and an edge region along its width. The thickness of the p-type doped layer 153 corresponding to the middle region is equal to the thickness of the p-type doped layer 153 corresponding to the edge region, and the doping concentration of the p-type doped layer 153 corresponding to the middle region is different from that of the p-type doped layer 153 corresponding to the edge region, thereby achieving different hole implantation capabilities. Specifically, the cross-sectional shape of the p-type doped layer 153 can be rectangular, so that its thickness in the gate width direction remains constant, and different hole implantation capabilities at different locations are achieved by different doping concentrations.
[0106] Preferably, in this embodiment, the doping concentration of the p-type doped layer 153 corresponding to the middle region is less than that of the p-type doped layer 153 corresponding to the edge region, so that the hole injection capability of the middle region is relatively weak, so as to avoid depleting the two-dimensional electron gas in part of the region, so that the on-resistance does not increase so much, thereby achieving the effect of relatively reducing the on-resistance.
[0107] Fifth embodiment
[0108] See Figures 12 to 15 This embodiment provides a semiconductor device 100, whose basic structure, principle and technical effects are the same as those of the first embodiment. For the sake of brevity, any parts not mentioned in this embodiment can be referred to the corresponding content in the first embodiment.
[0109] In this embodiment, the p-type doped layer 153 includes a plurality of p-type doped islands 159, which are uniformly spaced in the implantation region. A drain metal layer 151 is deposited in the region between two adjacent p-type doped islands 159 and partially covers the p-type doped islands 159. Each p-type doped island 159 extends towards both ends along the width direction of the implantation region and is exposed beyond the drain metal layer 151 to block the drain metal layer 151 on the p-type doped island 159 from the semiconductor stack 120. Specifically, in this embodiment, the p-type doped layer 153 is evenly distributed after being divided, and each p-type doped island 159 extends a drain metal layer 151 from both ends, which serves to adjust the edge electric field.
[0110] It should be noted that in this embodiment, the region with p-type doped islands 159 can realize hole injection, while the region without p-type doped islands 159 can be considered to have zero thickness of p-type doped layer 153, thereby realizing different hole injection capabilities at different locations in the injection region.
[0111] In this embodiment, the doping concentration of the multiple p-type doped islands 159 can be the same, which facilitates the one-time forming of the p-type doped islands 159.
[0112] In this embodiment, the drain metal layer 151 between two adjacent p-type doped islands 159 extends to both sides to form a field plate portion 158. By providing the field plate portion 158, which is spaced apart from the semiconductor stack 120, it is used to adjust the edge electric field of the implantation region. Specifically, the field plate portion 158 can be deposited on the dielectric layer 160, thereby being spaced a certain distance from the semiconductor stack 120 to achieve the field plate adjustment function.
[0113] It should be noted that in this embodiment, the projection of the field plate portion 158 on the semiconductor stack 120 does not overlap with the projection of the p-type doped island 159 on the semiconductor stack 120, so that the p-type doped island 159 and the field plate portion 158 can simultaneously play the function of adjusting the edge electric field, further solving the dynamic resistance problem, and at the same time, the on-resistance is not very large.
[0114] In this embodiment, the field plate portion 158 is integrally disposed on both sides of the drain metal layer 151, and the width of the drain metal layer 151 where the p-type doped islands 159 are disposed is smaller, so that the two ends of the p-type doped islands 159 can be exposed outside the drain metal layer 151.
[0115] This embodiment also provides a method for fabricating a semiconductor device 100. The basic steps, principles, and technical effects of this method are the same as in the first embodiment. For brevity, any parts not mentioned in this embodiment can be referred to the corresponding content in the first embodiment. The difference between this embodiment and the first embodiment lies in the formation of a p-type doped layer 153 and a drain metal layer 151.
[0116] See also Figures 16 to 18 In this embodiment, the steps of forming a gate 140 and a p-type doped layer 153 on the semiconductor stack 120 include: first forming a gate 140 on the semiconductor stack 120, depositing a p-type doped layer 153 in the implantation region of the semiconductor stack 120, and then etching the p-type doped layer 153 to divide the p-type doped layer 153 into a plurality of p-type doped islands 159.
[0117] Specifically, in the actual fabrication process, the gate 140 material and the p-type doped layer 153 can first be patterned on the surface of the semiconductor stack 120 to form multiple p-type doped islands 159. The materials of the p-type doped islands 159 and the gate 140 can be the same or different, and the multiple p-type doped islands 159 are spaced apart. Finally, source and drain metals can be formed again on the dielectric layer 160, wherein the drain metal layer 151 has a field plate portion 158 formed on the dielectric layer 160.
[0118] The semiconductor device 100 and its fabrication method provided in this embodiment of the invention involve setting a p-type doped layer 153 in the implantation region of a semiconductor stack 120, and then setting a drain metal layer 151 on the p-type doped layer 153 and the semiconductor stack 120. The drain metal layer 151 at least partially covers the p-type doped layer 153 and is in ohmic contact with the semiconductor stack 120. The p-type doped layer 153 is used to implant holes into the implantation region, and the thickness of the p-type doped layer 153 is different at different positions in the implantation region, thereby adjusting the hole implantation capability at different positions in the implantation region and adjusting the edge electric field of the implantation region. Compared to existing technologies, this embodiment achieves varying thicknesses at different locations by setting p-type doped islands 159, meaning that the thickness of the p-type doped layer 153 is zero in some areas. The p-type doped islands 159 can form PN junctions with the semiconductor stack 120 to generate holes, effectively injecting holes into the semiconductor stack 120. These holes can capture electrons that accidentally penetrate certain areas of the semiconductor due to the high electric field bombardment generated by the high voltage applied to the drain 150, thereby reducing the number of hot carrier electrons and their damage to the device. This suppresses the electric field at the edge of the drain 150, reducing resistance degradation and improving device reliability and dynamic behavior. Furthermore, because the thickness of the p-type doped layer 153 is zero in the areas between the p-type doped islands 159, the hole injection capability varies, preventing the depletion of the two-dimensional electron gas in some areas. This prevents a significant increase in on-resistance, achieving a relatively lower on-resistance and resulting in superior dynamic resistance and on-resistance performance.
[0119] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A semiconductor device, characterized in that, include: Substrate; Semiconductor stacks disposed on a substrate; and the source, gate, and drain electrodes disposed on the semiconductor stack; The drain electrode includes a drain metal layer and a p-type doped layer. The p-type doped layer is disposed in the implantation region of the semiconductor stack and is used to implant holes into the implantation region of the semiconductor stack. The doping concentration and / or thickness of the p-type doped layer are different at different positions in the implantation region to adjust the hole implantation capability at different positions in the implantation region and to adjust the edge electric field of the implantation region. The drain metal layer at least partially covers the p-type doped layer and is in ohmic contact with the semiconductor stack.
2. The semiconductor device according to claim 1, characterized in that, The implantation region has a middle region and an edge region along its width direction, and the thickness of the p-type doped layer corresponding to the middle region is different from the thickness of the p-type doped layer corresponding to the edge region.
3. The semiconductor device according to claim 2, characterized in that, The thickness of the p-type doped layer corresponding to the middle region is less than the thickness of the p-type doped layer corresponding to the edge region.
4. The semiconductor device according to claim 3, characterized in that, The p-type doped layer includes a first doped layer and a second doped layer. The first doped layer is disposed on the semiconductor stack, and the second doped layer is disposed on the first doped layer and at both edges of the first doped layer.
5. The semiconductor device according to claim 2, characterized in that, The implantation region has a middle region and an edge region along its width direction, and the thickness of the p-type doped layer corresponding to the middle region is greater than the thickness of the p-type doped layer corresponding to the edge region.
6. The semiconductor device according to claim 5, characterized in that, The doping concentration of the p-type doped layer corresponding to the middle region is less than the doping concentration of the p-type doped layer corresponding to the edge region.
7. The semiconductor device according to claim 1, characterized in that, The implantation region has a middle region and an edge region along its width direction. The thickness of the p-type doped layer corresponding to the middle region is equal to the thickness of the p-type doped layer corresponding to the edge region, and the doping concentration of the p-type doped layer corresponding to the middle region is different from the doping concentration of the p-type doped layer corresponding to the edge region.
8. The semiconductor device according to claim 1, characterized in that, The p-type doped layer includes a plurality of p-type doped islands, which are evenly spaced apart in the implantation region. The drain metal layer is deposited in the region between two adjacent p-type doped islands and partially covers the p-type doped islands. Each p-type doped island extends to both ends along the width direction of the implantation region and is exposed to the drain metal layer to block the drain metal layer on the p-type doped island from the semiconductor stack.
9. The semiconductor device according to claim 8, characterized in that, The drain metal layer between two adjacent p-type doped islands extends to both sides to form a field plate portion, which is spaced apart from the semiconductor stack and is used to adjust the edge electric field of the implantation region.
10. A method for fabricating a semiconductor device, applicable to the semiconductor device as described in any one of claims 1-9, characterized in that, The preparation method includes: Provide a substrate; A semiconductor stack is formed on the substrate; A gate and a p-type doped layer are formed on the semiconductor stack; Source and drain metal layers are formed on the semiconductor stack; The p-type doped layer is disposed in the implantation region of the semiconductor stack and is used to inject holes into the implantation region of the semiconductor stack. The doping concentration and / or thickness of the p-type doped layer are different at different positions in the implantation region to adjust the hole injection capability at different positions in the implantation region and to adjust the edge electric field of the implantation region. The drain metal layer at least partially covers the p-type doped layer and is in ohmic contact with the semiconductor stack.
Citation Information
Patent Citations
Semiconductor device and method for fabricating the same
CN101764063A
Semiconductor device and preparation method thereof
CN114759080A