A three-terminal parallel stacked double-sided photovoltaic cell and its preparation method

By connecting dye-sensitized solar cells with copper, zinc, tin, and sulfur solar cells in parallel, sharing the second gate wire electrode, forming a three-end parallel stacked double-sided photovoltaic cell, the problem of insufficient stability and efficiency of perovskite solar cells is solved. It has achieved improvement of photoelectric conversion efficiency and efficient application.

CN116417535BActive Publication Date: 2024-11-15YUNNAN NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310417085.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-11-15
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

The stability and service life of perovskite solar cells have not met the requirements of large-scale application industrialization, and the photoelectric conversion efficiency of single-junction dye-sensitized solar cells has not yet reached a satisfactory level. The photoelectric conversion efficiency needs to be improved to adapt to applications in special scenarios.

Method used

The dye-sensitized solar cells are connected in parallel with copper, zinc, tin, sulfur-type solar cells, and a second gate line electrode is used to form a three-end parallel stacked double-sided photovoltaic cell. The dye-sensitized solar cells with wide bandgap and copper, zinc, tin with narrow bandgap The advantages of sulfur solar cells are to expand the absorption range of sunlight and to avoid photocurrent characteristics matching problems through parallel structures.

Benefits of technology

It has achieved the improvement of photoelectric conversion efficiency, provided cheap and high-efficiency photovoltaic technology possibilities, is suitable for large-scale applications in the future, and avoided the limitation of photocurrent characteristics matching in series structures, and doubled the short-circuit current and significantly improved efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116417535B_ABST
    Figure CN116417535B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of solar cells, and specifically to a three-terminal parallel stacked double-sided photovoltaic cell and a preparation method thereof. A wide bandgap dye-sensitized solar cell is used as a top cell, and a narrow bandgap copper-zinc-tin-sulfur solar cell is used as a bottom cell. The bottom cell is stacked with a bottom cell soda-lime glass substrate, a first grid electrode, a window layer, a high resistance layer, a buffer layer, an absorption layer, and a second grid electrode in sequence; the top cell and the bottom cell share the second grid electrode, and are stacked with an electrolyte layer, a photoanode mesoporous layer, a transparent conductive layer, and a third grid electrode in sequence. This combination brings into play the respective advantages of dye-sensitized solar cells and copper-zinc-tin-sulfur solar cells, expands the absorption range of the sunlight spectrum, and provides the possibility for large-scale and high-efficiency application of cheap photovoltaic technology in the future, and has good application prospects in the field of solar cell technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and specifically to a three-terminal parallel stacked double-sided photovoltaic cell and a preparation method thereof. Background Art

[0002] In recent years, the most popular third-generation photovoltaic technology is perovskite solar cell technology. Its laboratory research and development efficiency has been significantly improved, but its stability and service life have not met the requirements for large-scale industrial application. The research on perovskite cell technology originated from the development of new dyes for dye-sensitized solar cells (DSSC). At present, the photoelectric conversion efficiency of single-junction dye-sensitized solar cells is close to 15%. Due to the simple preparation process, abundant raw materials and low preparation cost of dye-sensitized solar cells, they still have the potential for application in special scenarios. On the basis of the existing technology of dye-sensitized solar cells, it is of great significance to continue research and development to improve the photoelectric conversion efficiency. Summary of the invention

[0003] To solve the above problems, the present invention provides a three-terminal parallel stacked bifacial photovoltaic cell and a preparation method thereof. The core idea of ​​the present invention is to connect a dye-sensitized solar cell and a copper-zinc-tin-sulfur solar cell in parallel and share a second grid electrode to form a three-terminal parallel stacked bifacial photovoltaic cell. Both sides can receive sunlight and realize photoelectric conversion, thereby improving the overall photoelectric conversion efficiency of the device.

[0004] On the one hand, the present invention provides a three-terminal parallel stacked bifacial photovoltaic cell, comprising a bottom cell soda-lime glass substrate, a first grid electrode, a window layer, a high resistance layer, a buffer layer, an absorption layer, a second grid electrode, an electrolyte layer, a photoanode mesoporous layer, a transparent conductive layer, a third grid electrode, and a top cell glass substrate connected in sequence from one side to the other, wherein the second grid electrode serves as the positive electrode of the entire three-terminal parallel stacked bifacial photovoltaic cell, and the first grid electrode and the third grid electrode serve as the negative electrode of the entire three-terminal parallel stacked bifacial photovoltaic cell. The middle part of the first grid electrode and the second grid electrode constitutes a copper-zinc-tin-sulfur solar cell, and the middle part of the second grid electrode and the third grid electrode constitutes a dye-sensitized solar cell. The present invention provides a parallel stacked bifacial photovoltaic cell composed of a copper-zinc-tin-sulfur solar cell and a dye-sensitized solar cell in parallel.

[0005] Furthermore, the window layer is a Mo-doped ZnO film or an Al-doped ZnO film, the doping amount of Mo is 0.3-9wt.%, and the thickness of the ZnO film is 80-200 nanometers.

[0006] Furthermore, the high resistance layer is a ZnO film, and the thickness of the ZnO film is 30 to 60 nanometers.

[0007] Furthermore, the buffer layer is a Zn(S, O) film, and the thickness of the Zn(S, O) film is 20 to 50 nanometers.

[0008] Furthermore, the absorption layer is Cu2ZnSn(S x Se 1-x )4 thin film, Cu2ZnSn(S x Se 1-x )4 The band gap of the film is 0.9~1.2eV, Cu2ZnSn(S x Se 1-x )4The thickness of the film is 6000-10000 nanometers.

[0009] Furthermore, the photoanode mesoporous layer is a dye-loaded TiO2 mesoporous film, the band gap of the TiO2 mesoporous film is 3.3eV, the LUMO and HOMO energy level difference of the molecular orbital of the dye molecule is 1.6-1.9eV, and the thickness of the TiO2 mesoporous film is 8000-12000 nanometers.

[0010] In another aspect, the present invention provides a method for preparing a three-terminal parallel stacked bifacial photovoltaic cell, comprising the following steps:

[0011] Step 1: Prepare dye-sensitized solar cell photoanode;

[0012] Step 2: preparing copper-zinc-tin-sulfur solar cells;

[0013] Step 3: Assemble dye-sensitized solar cells and copper-zinc-tin-sulfur solar cells to form a three-terminal parallel stacked bifacial photovoltaic cell.

[0014] Furthermore, step 1 includes the following steps:

[0015] Prepare the cleaned top cell glass substrate;

[0016] The third gate electrode is prepared on the top cell glass substrate by using a masked electron beam evaporation method;

[0017] Depositing a transparent conductive layer on the surface of the third gate line electrode by using a radio frequency magnetron sputtering device;

[0018] The photoanode mesoporous layer is prepared on the transparent conductive layer by using a nanoparticle sol-gel coating method;

[0019] The prepared photoanode mesoporous layer is immersed in the dye solution for more than 24 hours until the dye fully loads the photoanode mesoporous layer to form a photoanode.

[0020] Furthermore, step 2 includes the following steps:

[0021] Prepare the cleaned bottom cell soda-lime glass substrate;

[0022] Depositing a first grid line electrode on the surface of the bottom cell soda-lime glass by using a masked electron beam evaporation method;

[0023] Depositing a window layer on the first gate electrode by radio frequency magnetron sputtering;

[0024] A high-resistance layer is deposited on the window layer by using a radio frequency magnetron sputtering method;

[0025] Use chemical water bath method or radio frequency double target co-sputtering ZnO and ZnS on the high resistance layer to form a buffer layer;

[0026] A Se-rich CZTSSe layer is deposited on the surface of the buffer layer by radio frequency magnetron co-sputtering technology or a pre-layer is electro-deposited and then selenized to form an absorption layer;

[0027] A second gate line electrode is deposited on the absorption layer.

[0028] Furthermore, step 3 includes the following steps:

[0029] The second gate electrode and the photoanode mesoporous layer are combined together by using an insulating resin package, and the distance between the two layers is 200 to 300 nanometers;

[0030] An electrolyte is injected between the second grid electrode and the photoanode mesoporous layer.

[0031] Beneficial effects of the present invention:

[0032] The present invention provides a three-terminal dye-sensitized solar cell and copper-zinc-tin-sulfur solar cell parallel stacked double-sided photovoltaic cell structure and a preparation method thereof, wherein a wide-bandgap dye-sensitized solar cell is used as a top cell, and a narrow-bandgap copper-zinc-tin-sulfur solar cell is used as a bottom cell. The bottom cell is sequentially stacked with a bottom cell soda-lime glass substrate, a first grid electrode, a window layer, a high-resistance layer, a buffer layer, an absorption layer and a second grid electrode; the top cell and the bottom cell share the second grid electrode, and are sequentially stacked with an electrolyte layer, a photoanode mesoporous layer, a transparent conductive layer and a third grid electrode. This combination brings into play the respective advantages of dye-sensitized solar cells and copper-zinc-tin-sulfur solar cells, expands the absorption range of the sunlight spectrum, and provides the possibility for large-scale and high-efficiency application of cheap photovoltaic technology in the future. In addition, the present invention adopts a parallel stacked structure with three terminals and two outputs, which avoids the disadvantage that the photocurrent characteristics of the two sub-cells that make up the conventional series stacked battery must be matched. The parallel connection can double the short-circuit current, fully utilize the efficiency of the two sub-cells, and effectively improve the photoelectric conversion efficiency of the entire parallel stacked battery. This provides a possible solution for the large-scale use of cheap and high-efficiency solar cells in the future.

[0033] Based on the above effects, the present invention has good application prospects in the field of solar cell technology.

[0034] The present invention will be further described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic diagram of the structure of a three-terminal parallel stacked bifacial photovoltaic cell. DETAILED DESCRIPTION

[0036] In order to make the objectives, technical solutions and advantages of the present application more clearly understood, the present application is further described in detail below with reference to the accompanying drawings and examples.

[0037] Example 1

[0038] like Figure 1 As shown, a three-terminal parallel stacked double-sided photovoltaic cell provided by the present invention includes a bottom cell soda-lime glass substrate, a first grid electrode, a window layer, a high resistance layer, a buffer layer, an absorption layer, a second grid electrode, an electrolyte layer, a photoanode mesoporous layer, a transparent conductive layer, a third grid electrode, and a top cell glass substrate connected in sequence from one side to the other. The second grid electrode serves as the positive electrode of the entire three-terminal parallel stacked double-sided photovoltaic cell, and the first grid electrode and the third grid electrode serve as the negative electrode of the entire three-terminal parallel stacked double-sided photovoltaic cell. In the present invention, a wide-bandgap dye-sensitized solar cell serves as the top cell, and a narrow-bandgap copper-zinc-tin-sulfur solar cell serves as the bottom cell. The present invention combines the top cell and the bottom cell, giving play to the respective advantages of the dye-sensitized solar cell and the copper-zinc-tin-sulfur solar cell, and improving the photoelectric conversion efficiency. The following is a detailed introduction to each layer of the three-terminal parallel stacked double-sided photovoltaic cell of the present invention:

[0039] (1) Bottom cell soda-lime glass substrate: The bottom cell soda-lime glass substrate adopts ordinary soda-lime glass substrate.

[0040] (2) First gate line electrode: The first gate line electrode is a nickel-aluminum alloy gate line electrode.

[0041] (3) Window layer: The window layer is a Mo-doped ZnO film or an Al-doped ZnO film, with the doping amount of Mo or Al being 0.3-9wt.%, and the thickness of the ZnO film being 80-200 nanometers. The window layer, as the N-type layer of the copper-zinc-tin-sulfur solar cell, allows more red light and near-infrared light to enter the absorption layer, while reflecting the minority carriers generated by the absorption layer, thereby improving the collection efficiency of photogenerated carriers.

[0042] (4) High resistance layer: The high resistance layer is a ZnO film with a thickness of 30 to 60 nanometers. The high resistance layer is used to increase the parallel resistance of copper-zinc-tin-sulfur solar cells to prevent internal leakage.

[0043] (5) Buffer layer: The buffer layer is a Zn(S, O) thin film with a thickness of 20 to 50 nanometers.O The ratio is 10 to 90%. The buffer layer is used to reduce the lattice mismatch between the high resistance layer and the absorption layer.

[0044] (6) Absorption layer: The absorption layer is Cu2ZnSn(S x Se 1-x )4 thin film, Cu2ZnSn(S x Se 1-x )4 The band gap of the film is 0.9~1.2eV, Cu2ZnSn(S x Se 1-x )4The thickness of the film is 6000-10000 nanometers. The absorption layer is used to absorb sunlight in the red and near-infrared spectral range. As the third-generation photovoltaic technology, copper zinc tin sulfur (CZTS) solar cells also have the advantages of abundant and cheap raw materials and relatively simple preparation process. Its research originated from the industrialized cadmium telluride solar cells and copper indium gallium selenide solar cells. Cadmium is toxic and indium gallium is rare and precious, so copper zinc tin sulfur thin film solar cells are very valuable for research. Although the photoelectric conversion efficiency prepared by its laboratory research has reached more than 13%, due to the large number of component elements in its absorption layer and the extremely difficult preparation of the pure phase structure, it is difficult to further improve the photoelectric conversion efficiency of copper zinc tin sulfur thin film solar cells. The absorption layer material of copper zinc tin sulfur selenium is a direct band gap semiconductor with an absorption coefficient of 10 4 cm -1 The absorption layer only needs to be 10 microns thick to absorb 90% of sunlight. The band gap width of CZTSe is 0.9eV, and the band gap width of CZTS is 1.5eV. Copper-zinc-tin-sulfur thin-film solar cells with a band gap width of 1eV can be prepared, which is very suitable as the bottom cell of the stacked solar cell.

[0045] (7) Second gridline electrode: The second gridline electrode serves as the counter electrode of the top cell and the positive electrode of the bottom cell, collecting electrons from the external circuit, catalyzing the reduction of the redox couple of the top cell, and collecting carrier holes from the absorption layer of the bottom cell. What is more creative is that the surface of the absorption layer of the bottom cell also has an excellent catalytic reduction effect on the redox couple of the top cell. The second gridline electrode is a composite counter electrode of a dye-sensitized solar cell. The second gridline electrode is a graphene gridline electrode doped with Pt or Ag, and the Pt or Ag doping amount is 0.3 to 16 wt.%; the Pt-doped graphene has an excellent catalytic reduction effect on the top cell; the Ag in the Ag-doped graphene gridline electrode has an excellent catalytic reduction effect on the absorption layer Cu2ZnSn(SxSe 1-x )4 has an optimization effect; further, the second gate line electrode is an Ag-doped graphene gate line electrode, in which Ag diffuses into the absorption layer, thereby enhancing the effect of the incident light and the absorption layer, improving the absorption of light by the absorption layer, and reducing defect recombination.

[0046] (8) Electrolyte layer: The electrolyte layer is an acetonitrile solution of LiI and I2. While the mesoporous layer of the photoanode is fully soaked, the relative distance between the counter electrode and the photoanode surface is 200-300 nanometers. The edges are encapsulated with a resin encapsulant, leaving only small holes. The electrolyte is injected from the small holes, specifically by vacuum dripping. The electrolyte is an acetonitrile solution with a LiI concentration of 0.3-0.5 mol / L and an I2 concentration of 0.03-0.05 mol / L. The electrolyte layer is a liquid electrolyte layer used to dissolve the redox couple and play the role of ion conduction. At the same time, its recombination speed with the electrons in the conduction band of the photoanode is slow, so that most of the electrons in the conduction band of the photoanode can flow to the external circuit.

[0047] (9) Photoanode mesoporous layer: The photoanode mesoporous layer is a TiO2 mesoporous film loaded with dyes. The band gap of the TiO2 mesoporous film is 3.3 eV, the molecular orbital energy difference of the dye is 1.6-1.9 eV, and the thickness of the TiO2 mesoporous film is 6000-10000 nanometers. The photoanode mesoporous layer is used to firmly adsorb the dye molecules, which are the light-absorbing materials of the top cell. When the dye molecules absorb short-wave photons, the internal electrons will be excited from the ground state to the excited state and injected into the conduction band of the TiO2 of the photoanode. The dye molecules used in the present invention are N719 dyes. The energy level difference between the HOMO energy level and the LUMO energy level of the N719 dye is about 1.7 eV. The dye-sensitized solar cell using the N719 dye is very suitable for the top cell of the tandem solar cell.

[0048] (10) Transparent conductive layer: The transparent conductive layer is a Ta-doped SnO2 thin film, the Ta doping amount is 0.3-9 wt.%, and the thickness is 80-200 nanometers. The transparent conductive layer is used to collect the conduction band electrons of the photoanode mesoporous layer.

[0049] (11) Third gate line electrode: The third gate line electrode is a nickel-aluminum alloy gate line electrode.

[0050] (12) Top cell glass substrate: The top cell glass substrate can be ordinary conventional glass or soda-lime glass.

[0051] At present, dye-sensitized solar cells or copper-zinc-tin-sulfur thin-film solar cells are usually used alone. The efficiency of the single-junction cells developed by the laboratory has not reached the photoelectric conversion efficiency comparable to the mainstream crystalline silicon solar cells that have been industrialized, and none of them exceeds 20%. At present, it is extremely difficult to achieve the industrialization requirements for large-scale applications by using them alone. The present invention combines two third-generation photovoltaic technologies to prepare a double-junction parallel stacked photovoltaic cell with a conversion efficiency of more than 20%.

[0052] In addition, in the present invention, sunlight incident from one side of the top cell or the bottom cell can penetrate the second grid line electrode and reach the bottom cell or the top cell on the other side, thereby enhancing the utilization of sunlight by the entire cell.

[0053] Example 2

[0054] The present invention also provides a method for preparing a three-terminal parallel stacked bifacial photovoltaic cell, the preparation method comprising the following steps:

[0055] Step 1: Prepare dye-sensitized solar cells;

[0056] Step 2: preparing copper-zinc-tin-sulfur solar cells;

[0057] Step 3: Assemble dye-sensitized solar cells and copper-zinc-tin-sulfur solar cells to form a three-terminal parallel stacked bifacial photovoltaic cell.

[0058] Wherein, step 1 comprises the following steps:

[0059] (1) Prepare a clean top cell glass substrate; the cleaning method is to place a glass substrate with a specification of 30*30 mm in acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 10 minutes, and then blow dry with a nitrogen gun.

[0060] (2) A third gate line electrode is prepared on the top cell glass substrate by using a masked electron beam evaporation method; specifically, a layer of Ni / Al gate line electrode with a thickness of 90 nanometers, a gate line width of 25 micrometers, and a gate line spacing of 0.2 centimeters is deposited on the glass substrate by using a screen printing sintering technique.

[0061] (3) A transparent conductive layer is deposited on the surface of the third gate line electrode using a radio frequency magnetron sputtering device; specifically, a layer of SnO2 film with a Ta doping amount of 2 wt.% and a thickness of 150 nm is deposited on the surface of the Ni / Al gate line electrode using radio frequency magnetron sputtering technology.

[0062] (4) A photoanode mesoporous layer is prepared on the transparent conductive layer by using a nanoparticle sol-gel coating method; specifically, TiO2 nanoparticles are coated on the surface of the Ta-doped SnO2 film by using a sol-gel method, and the nanocrystal particle size is 20 nanometers. After drying and sintering, a mesoporous TiO2 layer with a thickness of 8000 nanometers is formed.

[0063] (5) Immersing the prepared photoanode mesoporous layer in a dye solution for more than twelve hours until the dye fully loads the photoanode mesoporous layer to form a photoanode. Specifically, immersing in a polypyridyl ruthenium complex dye organic solvent solution for twelve hours to obtain a photoanode mesoporous layer loaded with N719 dye with a thickness of 8000 nanometers.

[0064] Wherein, step 2 comprises the following steps:

[0065] (1) Prepare a clean bottom cell soda-lime glass substrate; the cleaning method is to place the soda-lime glass with a specification of 30*30 mm in acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 10 minutes, and then blow dry with a nitrogen gun.

[0066] (2) Depositing a first gate electrode on the surface of the bottom cell soda-lime glass by masked electron beam evaporation; specifically, depositing a layer of Ni / Al gate electrode on the soda-lime glass substrate by screen printing sintering technology, with a thickness of 150 nanometers, a gate width of 25 micrometers, and a gate spacing of 0.2 centimeters.

[0067] (3) A window layer is deposited on the first gate electrode by radio frequency magnetron sputtering. Specifically, a layer of Al-doped ZnO film is deposited on a soda-lime glass substrate coated with a Ni / Al gate electrode by radio frequency magnetron sputtering technology, wherein the Al doping amount is 0.5 wt.%, and the thickness is 150 nm.

[0068] (4) A high-resistance layer is deposited on the window layer by radio frequency magnetron sputtering. Specifically, a ZnO high-resistance layer with a thickness of 30 nanometers is deposited on the Al-doped ZnO film by radio frequency magnetron sputtering.

[0069] (5) Using RF dual targets to co-sputter ZnO and ZnS on the high-resistance layer to form a buffer layer; specifically, using RF magnetron sputtering technology to co-sputter ZnS on the window layer 0.8 O 0.2 Buffer layer, thickness is 25 nanometers.

[0070] (6) Using RF magnetron co-sputtering technology on ZnS 0.8 O 0.2 Cu2ZnSn(S 0.1 Se 0.9 )4 layers with a thickness of 8000 nanometers. Depositing the buffer layer first and then the buffer layer is opposite to the conventional CZTSSe battery preparation process steps, which can reduce the sputtering damage of the later deposited buffer layer to the absorption layer.

[0071] (7) Depositing a second gate electrode on the absorption layer. Specifically, a Ag-doped graphene gate electrode is deposited on the surface of the absorption layer using screen printing and sintering technology, with a thickness of 200 nanometers, a gate width of 25 micrometers, and a gate spacing of 0.2 centimeters. During the sintering process, Ag ions diffuse into the absorption layer, which is beneficial to reducing the phase defects of the absorption layer.

[0072] Wherein, step 3 comprises the following steps:

[0073] (1) The Ag-doped graphene gate electrode and the mesoporous TiO2 layer are combined by using an insulating resin package, wherein the distance between the Ag-doped graphene gate electrode and the mesoporous TiO2 layer is in the range of 200 to 300 nanometers, and small holes are left to facilitate the injection of electrolyte;

[0074] (2) Inject electrolyte through the reserved small hole. Specifically, inject LiI and I2 acetonitrile solution between the counter electrode and the dye-loaded photoanode.

[0075] Example 3

[0076] Based on Example 2, step 1 includes the following steps:

[0077] (1) Prepare a clean top cell glass substrate; the cleaning method is to place a glass substrate with a specification of 20*20 mm in acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 10 minutes, and then blow dry with a nitrogen gun.

[0078] (2) A third gate line electrode is prepared on the top cell glass substrate by using a masked electron beam evaporation method; specifically, a layer of Ni / Al gate line electrode with a thickness of 60 nanometers, a gate line width of 25 micrometers, and a gate line spacing of 0.2 centimeters is deposited on the glass substrate by using a screen printing sintering technique.

[0079] (3) A transparent conductive layer is deposited on the surface of the third gate line electrode by using a radio frequency magnetron sputtering device; specifically, a Ta-doped SnO2 film is deposited on the surface of the Ni / Al gate line electrode by using radio frequency magnetron sputtering technology, with a doping amount of 7 wt.% and a thickness of 100 nanometers.

[0080] (4) A photoanode mesoporous layer is prepared on the transparent conductive layer by a nanoparticle sol-gel coating method; specifically, TiO2 nanoparticles are coated on the surface of the SnO2 film of Ta by a sol-gel method, and a mesoporous TiO2 layer with a thickness of 9500 nanometers is formed after drying and sintering.

[0081] (5) Immersing the prepared photoanode mesoporous layer in a dye solution for more than 24 hours until the dye fully loads the photoanode mesoporous layer to form a photoanode. Specifically, immersing in a polypyridyl ruthenium complex dye organic solvent solution for 12 hours to obtain a photoanode mesoporous layer loaded with the dye. The polypyridyl ruthenium complex dye includes dyes such as N3 and Z907.

[0082] Step 2 includes the following steps:

[0083] (1) Prepare a clean bottom cell soda-lime glass substrate; the cleaning method is to place a 20*20 mm soda-lime glass substrate in acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 10 minutes, and then blow dry it with a nitrogen gun.

[0084] (2) Depositing a first gate electrode on the surface of the bottom cell soda-lime glass by masked electron beam evaporation; specifically, depositing a layer of Ni / Al gate electrode on the soda-lime glass substrate by screen printing sintering technology, with a thickness of 80 nanometers, a gate width of 25 micrometers, and a gate spacing of 0.2 centimeters.

[0085] (3) A window layer is deposited on the first gate electrode by radio frequency magnetron sputtering. Specifically, a Mo-doped ZnO window layer is deposited on a soda-lime glass substrate coated with a Ni / Al gate electrode by radio frequency magnetron sputtering technology, wherein the Al doping amount is 5 wt.%, and the thickness is 60 nanometers.

[0086] (4) A high-resistance layer is deposited on the window layer by radio frequency magnetron sputtering. Specifically, a ZnO high-resistance layer with a thickness of 55 nanometers is deposited on the window layer by radio frequency magnetron sputtering technology.

[0087] (5) Using chemical water bath method or RF dual target co-sputtering ZnO and ZnS on the high resistance layer to form a buffer layer; specifically, using RF magnetron sputtering technology to co-sputter ZnS on the window layer 0.55 O 0.45 Buffer layer, thickness is 40 nanometers.

[0088] (6) Using electrochemical deposition prefabricated layer and then selenide sulfide technology on ZnS 0.55 O 0.45 Cu2ZnSn(S 0.3 Se 0.7 )4 layers with a thickness of 6500 nanometers. Depositing the buffer layer first and then the buffer layer is opposite to the conventional CZTSSe battery preparation process steps, which can reduce the sputtering damage of the later deposited buffer layer to the absorption layer.

[0089] (7) Depositing a second gate electrode on the absorption layer. Specifically, a Pt-doped graphene gate electrode is deposited on the surface of the absorption layer by screen printing and sintering technology, with a thickness of 75 nanometers, a gate width of 25 micrometers, and a gate spacing of 0.2 centimeters; further, in order to control production costs, a mixture of precious metal-free biochar and graphene is used to prepare the second gate electrode.

[0090] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A three-terminal parallel stacked bifacial photovoltaic cell, characterized in that: The invention comprises a bottom cell soda-lime glass substrate, a first grid electrode, a window layer, a high resistance layer, a buffer layer, an absorption layer, a second grid electrode, an electrolyte layer, a photoanode mesoporous layer, a transparent conductive layer, a third grid electrode, and a top cell glass substrate, which are sequentially connected from one side to the other side, wherein the second grid electrode serves as the positive electrode of the entire three-terminal parallel stacked bifacial photovoltaic cell, and the first grid electrode and the third grid electrode serve as the negative electrode of the entire three-terminal parallel stacked bifacial photovoltaic cell; wherein the high resistance layer is a ZnO thin film, the buffer layer is a Zn(S, O) thin film, and the absorption layer is a Cu2ZnSn(S x Se 1-x )4 film, the photoanode mesoporous layer is a dye-loaded TiO2 mesoporous film, and the second grid line electrode is an Ag-doped graphene grid line electrode prepared by screen printing and sintering technology.

2. The three-terminal parallel stacked bifacial photovoltaic cell according to claim 1, characterized in that: The window layer is a Mo-doped ZnO film or an Al-doped ZnO film, the Mo doping amount is 0.3-9wt.%, and the thickness of the ZnO film is 80-200 nanometers.

3. The three-terminal parallel stacked bifacial photovoltaic cell according to claim 1, characterized in that: The thickness of the high resistance layer is 30-60 nanometers.

4. The three-terminal parallel stacked bifacial photovoltaic cell according to claim 1, characterized in that: The thickness of the Zn(S, O) film is 20-50 nanometers.

5. The three-terminal parallel stacked bifacial photovoltaic cell according to claim 4, characterized in that: The Cu2ZnSn(S x Se 1-x )4 film has a band gap of 0.9~1.2eV, and the Cu2ZnSn(S x Se 1-x )4The thickness of the film is 6000-10000 nanometers.

6. The three-terminal parallel stacked bifacial photovoltaic cell according to claim 1, characterized in that: The band gap of the TiO2 mesoporous film is 3.3 eV, the energy level difference between LUMO and HOMO of the molecular orbital of the dye molecule is 1.6-1.9 eV, and the thickness of the TiO2 mesoporous film is 8000-12000 nanometers.

7. The method for preparing a three-terminal parallel stacked bifacial photovoltaic cell according to any one of claims 1 to 6, characterized in that: The steps include: Step 1: Prepare dye-sensitized solar cell photoanode; Step 2: preparing copper-zinc-tin-sulfur solar cells; Step 3: Assemble the dye-sensitized solar cells and copper-zinc-tin-sulfur solar cells to form a three-terminal parallel stacked bifacial photovoltaic cell; Wherein, the step 1 comprises the following steps: Prepare the cleaned top cell glass substrate; The third gate electrode is prepared on the top cell glass substrate by using a masked electron beam evaporation method; Depositing a transparent conductive layer on the surface of the third gate line electrode by using a radio frequency magnetron sputtering device; The photoanode mesoporous layer is prepared on the transparent conductive layer by using a nanoparticle sol-gel coating method; Immersing the prepared photoanode mesoporous layer in a dye solution for more than 24 hours until the dye is fully loaded in the photoanode mesoporous layer to form a photoanode; The step 2 comprises the following steps: Prepare the cleaned bottom cell soda-lime glass substrate; Depositing a first grid line electrode on the surface of the bottom cell soda-lime glass by using a masked electron beam evaporation method; Depositing a window layer on the first gate electrode by radio frequency magnetron sputtering; A high-resistance layer is deposited on the window layer by using a radio frequency magnetron sputtering method; Use chemical water bath method or radio frequency double target co-sputtering ZnO and ZnS on the high resistance layer to form a buffer layer; A Se-rich CZTSSe layer is deposited on the surface of the buffer layer by radio frequency magnetron co-sputtering technology to form an absorption layer; Depositing a second gate line electrode on the absorption layer, wherein the second gate line electrode is an Ag-doped graphene gate line electrode prepared by screen printing and sintering technology; The step 3 comprises the following steps: The second gate line electrode and the photoanode mesoporous layer are sealed together by insulating resin; An electrolyte is injected between the second grid electrode and the photoanode mesoporous layer.