wound core
By controlling the frequency of subgrain boundaries and the radius of curvature of the bends in the wound core, the problem of uneven core efficiency in the manufacturing of wound cores was solved, and more efficient core performance was achieved.
Patent Information
- Application Number
- CN202180072386.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-26
- Filing Date
- 2021-10-26
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2041-10-26
AI Technical Summary
In the process of manufacturing wound iron cores, even though steel plates with crystal orientation control are used as raw materials, the efficiency of the iron cores still varies, mainly due to the unevenness of the degree of iron loss deterioration during bending.
By bending and stacking directional electromagnetic steel sheets under specific manufacturing conditions, the frequency of subgrain boundaries and the inner side curvature radius of the bend are controlled to form a rectangular wound core with a 90° angle, thus suppressing the deterioration of core efficiency.
It effectively suppressed the deterioration of core efficiency caused by carelessness, and improved the overall performance and stability of the core.
Smart Images

Figure CN116419978B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a wound core. This application claims priority based on Japanese Patent Application No. 2020-178553, filed on October 26, 2020, the contents of which are incorporated herein by reference. Background Technology
[0002] Directional electromagnetic steel sheets are steel sheets containing less than 7% by mass of Si and exhibiting a secondary recrystallization texture with secondary recrystallized grains aggregated in the {110}<001> orientation (Goss orientation). The magnetic properties of directional electromagnetic steel sheets are significantly affected by the degree of aggregation in the {110}<001> orientation. In recent years, practical directional electromagnetic steel sheets have been controlled by ensuring that the angle between the <001> direction of the crystal and the rolling direction falls within a range of approximately 5°.
[0003] Directional electromagnetic steel sheets are used in transformer cores and other applications through stacking, but high magnetic flux density and low iron loss are required as key magnetic properties. It is known that crystal orientation is closely related to these properties; for example, precise orientation control techniques, such as those disclosed in Patent Documents 1-3, have been developed.
[0004] In directional electromagnetic steel sheets, the boundaries of the aforementioned crystal orientations are recognized as grain boundaries, and the behavior of grain boundary movement used to control crystal orientation is being studied in greater depth. However, there are not many techniques for improving properties by controlling the subgrain boundaries (small-angle grain boundaries, small-tilt grain boundaries) formed by the specific configuration of tiny dislocations existing within the grains, to the extent disclosed in patent documents 4 to 7.
[0005] In addition, the manufacturing of wound iron cores is a well-known method, such as that described in Patent Document 8: after the steel plate is rolled into a cylindrical shape, it is pressed while keeping the cylindrical laminate unchanged, so that the corners have a constant curvature. After being formed into a roughly rectangular shape, stress is relieved and the shape is maintained by annealing.
[0006] On the other hand, as another manufacturing method for wound iron cores, patent documents 9-11 disclose techniques. In this technique, the steel plate portion at the corner of the wound iron core is pre-bent to form a small bending region with an inner side curvature radius of less than 5 mm, and the bent steel plates are stacked to form the iron core. According to this manufacturing method, the large pressing process as in the past is not required, the steel plate can be precisely bent to maintain the shape of the iron core, and since the processing strain is concentrated only in the bending portion (corner), the stress relief using the aforementioned annealing process can be omitted, resulting in significant industrial advantages and developing applications.
[0007] Existing technical documents
[0008] Patent documents
[0009] Patent Document 1: Japanese Patent Application Publication No. 2001-192785
[0010] Patent Document 2: Japanese Patent Application Publication No. 2005-240079
[0011] Patent Document 3: Japanese Patent Application Publication No. 2012-052229
[0012] Patent Document 4: Japanese Patent Application Publication No. 2004-143532
[0013] Patent Document 5: Japanese Patent Application Publication No. 2006-219690
[0014] Patent Document 6: Japanese Patent Application Publication No. 2001-303214
[0015] Patent Document 7: International Publication No. 2020 / 027215
[0016] Patent Document 8: Japanese Patent Application Publication No. 2005-286169
[0017] Patent Document 9: Japanese Patent No. 6224468
[0018] Patent Document 10: Japanese Patent Application Publication No. 2018-148036
[0019] Patent Document 11: Australian Patent Application Publication No. 2012337260 Summary of the Invention
[0020] The problem that the invention aims to solve
[0021] The inventors have conducted a detailed study on the efficiency of transformer cores manufactured by the following method. In this method, steel sheets are pre-bent to form a relatively small bending region with an inner side curvature radius of 5 mm or less, and the bent steel sheets are stacked to form a wound core. As a result, it was recognized that even when using steel sheets with approximately equal control over crystal orientation and approximately equal magnetic flux density and iron loss measured on a single sheet as raw materials, differences in core efficiency sometimes occur.
[0022] The cause was investigated, and it was speculated that the efficiency difference that caused the problem was due to the difference in the degree of iron loss degradation of each raw material during bending.
[0023] Based on this perspective, various steel plate manufacturing conditions and core shapes were studied, and their effects on core efficiency were categorized. The results showed that by using steel plates manufactured under specific conditions as raw materials for cores of specific sizes and shapes, it is possible to control the core efficiency to achieve the optimal efficiency commensurate with the magnetic properties of the steel plate raw materials.
[0024] The present invention was made in view of the above-mentioned problems, and its object is to provide a wound core that improves the efficiency of the core by pre-bending a steel plate to form a relatively small bending area with an inner side curvature radius of less than 5 mm and stacking the bent steel plate to form a wound core, in order to suppress the deterioration of the core efficiency caused by accident.
[0025] Methods for solving problems
[0026] To achieve the above objectives, one embodiment of the present invention relates to a wound iron core, which is a wound iron core body having a generally rectangular shape when viewed from the side, characterized in that:
[0027] In the main body of the wound iron core, the first flat portion and the corner portion are continuously alternately arranged in the length direction, including a portion formed by stacking directional electromagnetic steel plates in the thickness direction by two adjacent first flat portions sandwiching each corner portion at an angle of 90°, and having a stacked structure that is roughly rectangular in shape when viewed from the side.
[0028] Each corner portion, in a side view of the directional electromagnetic steel plate, has two or more curved portions with a curved shape, and a second flat portion is provided between adjacent curved portions, and the total curvature angle of each curved portion in a corner portion is 90°.
[0029] The inner side curvature radius r of the curved portion in the side view is more than 1 mm and less than 5 mm;
[0030] In the directional electromagnetic steel plate,
[0031] Its chemical composition, expressed in % by mass, contains:
[0032] Si: 2.0–7.0%
[0033] The remaining portion includes Fe and impurities.
[0034] It has a texture oriented towards the Goss orientation, and
[0035] In one or more of the first planar portions and the second planar portions adjacent to at least one of the curved portions, the frequency of the presence of subgrain boundaries in a region within 9 mm in a direction perpendicular to the boundary of the curved portion satisfies the following equation (1).
[0036] (Nac+Nal) / Nt≥0.010 (1)
[0037] Here, Nt in equation (1) is: the total number of line segments connecting two adjacent measurement points in the parallel and vertical directions of the boundary of the curved portion when multiple measurement points are arranged at 2mm intervals in the region of the first plane portion or the second plane portion adjacent to the curved portion.
[0038] In Equation (1), Nac is the number of line segments in the direction parallel to the boundary of the curved portion that can identify subgrain boundaries, and Nal in Equation (1) is the number of line segments in the direction perpendicular to the boundary of the curved portion that can identify subgrain boundaries.
[0039] Furthermore, in one embodiment of the present invention, in one or more of the first planar portion and the second planar portion adjacent to at least one of the curved portions, the following formula (2) may also be satisfied.
[0040] (Nac+Nal) / (Nbc+Nbl)>0.30 (2)
[0041] Here, Nbc in equation (2) is the number of line segments in the direction parallel to the boundary of the curved portion that can identify grain boundaries other than the subgrain boundary, and Nbl in equation (2) is the number of line segments in the direction perpendicular to the boundary of the curved portion that can identify grain boundaries other than the subgrain boundary.
[0042] Furthermore, in one embodiment of the present invention, in one or more of the first planar portion and the second planar portion adjacent to at least one of the curved portions, the following formula (3) may also be satisfied.
[0043] Nal / Nac≥0.80 (3)
[0044] Furthermore, in one embodiment of the present invention, the chemical composition of the directional electromagnetic steel plate, expressed as a percentage by mass, may also contain:
[0045] Si: 2.0–7.0%
[0046] Nb: 0~0.030%
[0047] V: 0~0.030%
[0048] Mo: 0–0.030%
[0049] Ta: 0~0.030%
[0050] W: 0~0.030%
[0051] C: 0~0.0050%
[0052] Mn: 0~1.0%
[0053] S: 0~0.0150%
[0054] Se: 0~0.0150%
[0055] Al: 0~0.0650%
[0056] N: 0~0.0050%
[0057] Cu: 0–0.40%
[0058] Bi: 0~0.010%
[0059] B: 0~0.080%
[0060] P: 0–0.50%
[0061] Ti: 0~0.0150%
[0062] Sn: 0-0.10%
[0063] Sb: 0~0.10%
[0064] Cr: 0–0.30%, and
[0065] Ni: 0~1.0%,
[0066] The remainder includes Fe and impurities.
[0067] Furthermore, in one embodiment of the present invention, the chemical composition of the directional electromagnetic steel sheet may also contain a total of 0.0030 to 0.030% by mass of at least one of Nb, V, Mo, Ta, and W.
[0068] Invention Effects
[0069] According to the present invention, in a wound iron core formed by stacking layers of bent steel plates, the deterioration of iron core efficiency caused by carelessness can be effectively suppressed. Attached Figure Description
[0070] Figure 1 This is a perspective view schematically illustrating one embodiment of the wound iron core involved in the present invention.
[0071] Figure 2 yes Figure 1 The side view of the wound iron core shown in the embodiment.
[0072] Figure 3 This is a side view schematically illustrating another embodiment of the wound iron core involved in the present invention.
[0073] Figure 4 This is a side view schematically showing an example of a single layer of directional electromagnetic steel sheet constituting the wound iron core of the present invention.
[0074] Figure 5 This is a side view schematically showing another example of a single layer of directional electromagnetic steel sheet constituting the wound iron core of the present invention.
[0075] Figure 6 This is a side view schematically showing an example of a curved portion of the directional electromagnetic steel sheet constituting the wound iron core of the present invention.
[0076] Figure 7 This is a diagram used to schematically illustrate the offset angles (α, β, γ) associated with the crystal orientation observed in a directional electromagnet.
[0077] Figure 8 This is a schematic diagram showing the dimensional parameters of the wound iron core manufactured according to the embodiment.
[0078] Figure 9 This is a grid diagram used to illustrate the configuration method of measurement points for a specific grain boundary in this embodiment. Detailed Implementation
[0079] The wound iron core according to one embodiment of the present invention will now be described in detail. However, the present invention is not limited to the configuration disclosed in this embodiment, and various modifications can be made without departing from the spirit of the present invention. Furthermore, in the numerical ranges described below, the lower and upper limits are included within the range. Values expressed as "more than" or "less than" are not included in the numerical range. In addition, the "%" in relation to chemical composition means "mass %" unless otherwise specified.
[0080] Furthermore, terms such as “parallel,” “perpendicular,” “identical,” “right angle,” etc., used to determine the shape or geometric conditions and their degree as described in this specification, or values of length, angle, etc., are not limited to a strict meaning, but are interpreted to include a range of degrees to which the same function can be expected.
[0081] In addition, in this specification, "directional electromagnetic steel plate" is sometimes simplified to "steel plate" or "electromagnetic steel plate", and "wound iron core" is simplified to "iron core".
[0082] This embodiment relates to a wound iron core, which is a wound iron core body that is generally rectangular in shape when viewed from the side. The wound iron core is characterized in that:
[0083] The wound core body comprises a portion consisting of directional electromagnetic steel plates stacked in the thickness direction, which are alternately continuous in the length direction by first planar portions and corner portions, with an angle of 90° between two adjacent first planar portions sandwiching each corner portion, and has a stacked structure that is roughly rectangular in shape when viewed from the side.
[0084] Each corner portion, in a side view of the directional electromagnetic steel plate, has two or more curved portions with a curved shape, and a second flat portion is provided between adjacent curved portions, and the total curvature angle of each curved portion in a corner portion is 90°.
[0085] The inner side curvature radius r of the curved portion in the side view is more than 1 mm and less than 5 mm;
[0086] In the directional electromagnetic steel plate,
[0087] Its chemical composition, expressed in % by mass, contains:
[0088] Si: 2.0–7.0%
[0089] The remaining portion includes Fe and impurities.
[0090] It has a texture oriented towards the Goss orientation, and
[0091] In one or more of the first planar portions and the second planar portions adjacent to at least one of the curved portions, the frequency of the presence of subgrain boundaries in a region within 9 mm in a direction perpendicular to the boundary of the curved portion satisfies the following equation (1).
[0092] (Nac+Nal) / Nt≥0.010 (1)
[0093] Here, Nt in equation (1) is: the total number of line segments connecting two adjacent measurement points in the parallel and vertical directions of the boundary of the curved portion when multiple measurement points are arranged at 2mm intervals in the region of the first plane portion or the second plane portion adjacent to the curved portion.
[0094] In Equation (1), Nac is the number of line segments in the direction parallel to the boundary of the curved portion that can identify subgrain boundaries, and Nal in Equation (1) is the number of line segments in the direction perpendicular to the boundary of the curved portion that can identify subgrain boundaries.
[0095] 1. Shape of the wound iron core and directional electromagnetic steel sheet
[0096] First, the shape of the wound core in this embodiment will be described. The shapes of the wound core and the directional electromagnetic steel plate described here are not particularly novel. For example, they are simply referenced to the shapes of the wound core and the directional electromagnetic steel plate known in the background art as described in Patent Documents 9 to 11.
[0097] Figure 1 This is a perspective view schematically illustrating one embodiment of a wound iron core. Figure 2 yes Figure 1 A side view of the wound iron core shown in the embodiment. Furthermore, Figure 3 This is a side view schematically illustrating another embodiment of the wound iron core.
[0098] Furthermore, in this embodiment, "side view" refers to the view along the width of the long strip of directional electromagnetic steel plate that constitutes the wound core. Figure 1 Looking at the Y-axis direction, a side view is a diagram that shows the shape as seen from the side. Figure 1 (Graph of the Y-axis direction).
[0099] The wound core according to this embodiment has a wound core body 10 that is generally rectangular (generally polygonal) in shape when viewed from the side. The wound core body 10 is formed by stacking directional electromagnetic steel plates 1 in the thickness direction, and has a stacked structure 2 that is generally rectangular in shape when viewed from the side. The wound core body 10 can also be used directly as a wound core. In order to fix the stacked multiple directional electromagnetic steel plates 1 as a whole, known fasteners such as cable ties can also be provided as needed.
[0100] In this embodiment, the length of the core of the wound core body 10 is not particularly limited. Even if the core length varies, the iron loss occurring in the bending portion 5 is fixed because the volume of the bending portion 5 is constant. Since a longer core length reduces the volume ratio of the bending portion 5 relative to the wound core body 10, the impact on iron loss degradation is also smaller. Therefore, a longer core length of the wound core body 10 is preferable. Preferably, the core length of the wound core body 10 is 1.5 m or more, more preferably 1.7 m or more. Furthermore, in this embodiment, the core length of the wound core body 10 refers to the circumference at the center point in the stacking direction of the wound core body 10 when viewed from the side.
[0101] The wound core of this embodiment is suitable for any application known in the past.
[0102] like Figure 1 and 2As shown, in the wound core body 10, the first planar portion 4 and the corner portion 3 are alternately continuous in the length direction, and include portions formed by stacking directional electromagnetic steel plates 1 in the thickness direction by two first planar portions 4 adjacent to each corner portion 3 at an angle of 90°, having a stacked structure 2 that appears roughly rectangular in side view. Furthermore, in this specification, "first planar portion" and "second planar portion" are sometimes simplified to "planar portion" respectively.
[0103] Viewed from the side, each corner portion 3 of the directional electromagnetic steel plate 1 has two or more curved portions 5, and the total curvature angle of each curved portion 5 in a corner portion 3 is 90°. The corner portion 3 has a second flat portion 4a between adjacent curved portions 5. Therefore, the corner portion 3 is configured to have two or more curved portions 5 and one or more second flat portions 4a.
[0104] Figure 2 One implementation is that there are two curved portions 5 in one corner portion 3. Figure 3 One implementation is that there are three curved parts 5 in one corner part 3.
[0105] As these examples illustrate, in this embodiment, a corner may be composed of two or more bends, but from the perspective of suppressing iron loss by suppressing strain caused by deformation during processing, it is preferable that the bending angle Φ of the bend 5 is 60° or less. Specifically, for example... Figure 3 Φ1, Φ2, and Φ3 are preferably 60° or less, and more preferably 45° or less.
[0106] It has two bends at one corner. Figure 2 In some implementations, to reduce iron loss, the angle can be specified as Φ1 = 60° and Φ2 = 30°, or Φ1 = 45° and Φ2 = 45°. Furthermore, a corner section may have three bends. Figure 3 In this implementation, from the perspective of reducing iron loss, for example, Φ1 = 30°, Φ2 = 30°, and Φ3 = 30° can be specified. Furthermore, from the perspective of production efficiency, it is preferable that the bending angles (bending angles) are equal. Therefore, in the case where one corner has two bends, it is preferable that Φ1 = 45° and Φ2 = 45°. Moreover, in the case where one corner has three bends... Figure 3 In the implementation of the method, from the point of reducing iron loss, it is preferred, for example, that Φ1 = 30°, Φ2 = 30° and Φ3 = 30°.
[0107] Reference Figure 6 A more detailed explanation of the curved section 5 will follow. Figure 6This is a schematic illustration of an example of a curved portion (curved section) of a directional electromagnetic steel sheet. The bending angle of the curved portion 5 refers to the angle difference between the straight section on the rear side and the straight section on the front side of the curved portion 5 in the bending direction. It is represented by the supplementary angle Φ formed by extending the straight sections of the plane portions 4 and 4a on both sides of the curved portion 5 outside the directional electromagnetic steel sheet 1. The point where the extended straight line leaves the surface of the steel sheet is the boundary between the plane portions 4 and 4a on the outer surface of the steel sheet and the curved portion 5. Figure 6 In the middle, points F and G are points F and G respectively.
[0108] Furthermore, straight lines perpendicular to the outer surface of the steel plate are extended from points F and G respectively, and their intersections with the inner surface of the steel plate are designated as points E and D. These points E and D represent the boundaries between the planar portions 4 and 4a and the curved portion 5 on the inner surface of the steel plate.
[0109] In addition, the so-called curved portion 5 in this embodiment refers to the part of the directional electromagnetic steel plate 1 that is surrounded by the aforementioned points D, E, F, and G in a side view of the directional electromagnetic steel plate 1. Figure 6 In the diagram, the inner surface of the steel plate between point D and point E, i.e., the curved part 5, is denoted as La, and the outer surface of the steel plate between point F and point G, i.e., the curved part 5, is denoted as Lb.
[0110] Furthermore, in this embodiment, the radius of curvature r of the inner surface of the curved portion 5 is defined in the side view of the curved portion 5. Figure 6For example, the method for determining the inner surface curvature radius r of the curved portion 5 will be specifically explained. Initially, in the planar portions 4 and 4a sandwiching the curved portion 5, straight lines that are at least 1 mm in contact with the surface of the planar portion, i.e., the straight portion, are determined. These straight lines are respectively designated as imaginary lines Lb-elongation1 and Lb-elongation2, and the intersection point is designated as point B. Ideally, the lengths of line segments BF and BG are the same, but in reality, due to deviations in processing conditions and unavoidable variations, there are sometimes some differences. In such cases, in order to properly evaluate the effects of the present invention, points F' and G' are determined from points B, F, and G. In other words, let LL be the distance between the longer of line segments BF and BG (for example, let BG be longer than BF). Let F' be the point on the imaginary line Lb-elongation1 that moves from point B towards point F only a distance of LL, and let G' be the point on the imaginary line Lb-elongation2 that moves from point B towards point G only a distance of LL. At this point, either F' or G' will coincide with the original point F or point G (for example, when BG is longer than BF, point G' will coincide with the original point G).
[0111] Furthermore, when the lengths of line segment BF and line segment BG are equal, Figure 6 In the above, point F′ is the same as the original point F. Correspondingly, point E′, as described below, is the same as the original point E.
[0112] Furthermore, when the lengths of line segment BF and line segment BG are different, straight lines perpendicular to the outer surface of the steel plate are extended from points F' and G' respectively, and the intersection of the two lines is set as the curvature center A. Also, the intersections of line segments AF' and AG' with the inner surface La of the steel plate are set as points E' and D' respectively. In this case, the circle centered at point A and passing through points E' and D' approximates the curved surface of the curved portion 5 in this embodiment, and the length of line segment AE' (which is the same as the length of line segment AD') is the inner surface curvature radius r in this embodiment. The smaller the inner surface curvature radius r, the greater the curvature of the curved portion of the curved portion 5; the larger the inner surface curvature radius r, the less curvature of the curved portion of the curved portion 5.
[0113] In the wound core of this embodiment, the inner side curvature radius r of each bent portion 5 of each directional electromagnetic steel plate 1 stacked in the thickness direction may vary to some extent. This variation may sometimes be due to variations in forming accuracy, or it may be considered an unintentional variation caused by processing during stacking. Such unintentional errors can be controlled to around 0.3 mm or less in typical industrial manufacturing. In cases of large variations, a representative value can be obtained by measuring the inner side curvature radius r of a sufficient number of steel plates and averaging the measured values. Furthermore, it is possible to intentionally change the inner side curvature radius for some reason; this embodiment does not exclude such a method.
[0114] Furthermore, in this embodiment, as described above, it is assumed that line segments BF and BG have different lengths, and the bending process is asymmetrical. In this situation, it is considered that the bending should be locally concentrated in the region on the side with the shorter line segment length, and that the effects of the invention can be more effectively achieved on that side. However, the subgrain boundary measurement, described later, need not be performed on the planar portion on the side with the shorter line segment length, regardless of whether the bending process is asymmetrical or symmetrical. This is because it is clear that even if the strain extends outwards from the bent portion on the side with the longer line segment length, the effects of the invention can still be achieved in that region.
[0115] Furthermore, there are no particular limitations on the method for observing the shape of the curved portion 5 and the method for measuring the inner surface curvature radius r. For example, a commercially available microscope (Nikon ECLIPSE LV150) can be used to observe and measure it at 15 to 200x magnification. Here, in order to determine the planar portions 4 and 4a, it is best to take pictures at low magnification to observe a large area. In addition, when determining the inner surface curvature radius r, it is best to take pictures at high magnification and increase the number of pictures to form a series of photographs. Furthermore, when calculating the inner surface curvature radius r, if there is a concern about measurement errors when taking pictures at low magnification, it is necessary to magnify the pictures for measurement.
[0116] In this embodiment, by specifying the inner side curvature radius r of the bent portion 5 within the range of 1 mm or more and 5 mm or less, and by using a specific directional electromagnetic steel plate with a friction coefficient controlled as described below, the noise of the wound core can be controlled. Preferably, the inner side curvature radius r of the bent portion 5 is 3 mm or less. In this case, the effect of this embodiment can be more significantly achieved.
[0117] Furthermore, it is most preferred that all the bent portions 5 within the iron core satisfy the inner surface curvature radius r specified in this embodiment. When there are bent portions 5 that satisfy the inner surface curvature radius r of this embodiment and bent portions 5 that do not satisfy it, it is preferred that at least half of the bent portions 5 satisfy the inner surface curvature radius r specified in this embodiment.
[0118] Figure 4 and Figure 5 This is a schematic illustration of an example of a layer of directional electromagnetic steel plate 1 wound in the main body 10 of the iron core. (See diagram below.) Figure 4 and Figure 5 As shown in the example, the directional electromagnetic steel plate 1 used in this embodiment is formed by bending and has a corner portion 3 composed of two or more bending portions 5 and a first flat portion 4. It forms a ring that is approximately rectangular in side view through one or more end faces, i.e. joint portions 6, in the length direction of the directional electromagnetic steel plate 1.
[0119] In this embodiment, the wound core body 10 only needs to have a stacked structure 2 that is roughly rectangular in shape when viewed from the side. For example... Figure 4 As shown in the example, a single layer of wound iron core body 10 can also be formed from a single directional electromagnetic steel plate 1 via a single joint 6 (that is, each roll is connected to a single directional electromagnetic steel plate 1 via a single joint 6), as... Figure 5 As shown in the example, a wound core of about half a turn can also be formed by one directional electromagnetic steel plate 1, and a wound core body 10 can be formed by two directional electromagnetic steel plates 1 via two joints 6 (that is, each roll connects two directional electromagnetic steel plates 1 to each other via two joints 6).
[0120] The thickness of the directional electromagnetic steel plate 1 used in this embodiment is not particularly limited and can be appropriately selected according to the application, but it is usually in the range of 0.15mm to 0.35mm, preferably in the range of 0.18mm to 0.23mm.
[0121] 2. Composition of directional electromagnetic steel plates
[0122] Next, the configuration of the directional electromagnetic steel plate 1 constituting the main body 10 of the wound iron core will be described. In this embodiment, the presence frequency of the subgrain boundaries of the planar portions 4, 4a adjacent to the curved portions 5 of the adjacently stacked electromagnetic steel plates and the arrangement position of the electromagnetic steel plates within the iron core that controls the presence frequency of the subgrain boundaries are characterized.
[0123] (1) Presence frequency of subgrain boundaries in the planar portion adjacent to the curved portion
[0124] The directional electromagnetic steel plate 1 constituting the wound core of this embodiment is controlled by increasing the presence frequency of subgrain boundaries of the stacked steel plates, at least in a portion of the bend. If the presence frequency of subgrain boundaries near the bend 5 decreases, the effect of avoiding efficiency degradation in the core having the core shape of this embodiment is not exhibited. In other words, it means that efficiency degradation is easily suppressed by arranging subgrain boundaries near the bend 5.
[0125] The mechanism behind this phenomenon is not entirely clear, but it can be considered as follows.
[0126] In this embodiment, the macroscopic strain (deformation) caused by bending of the iron core is confined to a very narrow region, namely within the bending portion 5. However, if elastic strain accompanied by micro-strain and plastic strain occurs, from the perspective of the crystal structure inside the steel plate, it can be considered that the dislocations formed in the bending portion 5 move and expand outwards towards the plane portions 4 and 4a of the bending portion 5. It is known that the dispersion of dislocations into the crystal due to general plastic deformation significantly deteriorates iron loss. At this time, if subgrain boundaries are arranged near the bending portion 5, so that the subgrain boundaries function as obstacles (dislocation vanishing points) or buffer zones for elastic strain to prevent the movement of dislocations towards the plane portions 4 and 4a, the dispersion area of dislocations and elastic strain caused by deformation can be kept near the bending portion 5. This embodiment believes that the decrease in iron core efficiency can be suppressed through this effect. It should be noted here that the relatively large number of dispersed subgrain boundaries in this embodiment are also basically formed by a special arrangement of dislocations. The above describes how dislocations caused by deformation significantly degrade iron losses. However, it is possible to consider configuring dislocations that form subgrain boundaries in a way that eliminates minute orientation differences within the grains and mitigates stress caused by accident. In this regard, it is believed that as long as the amount of subgrain boundaries is moderate, there is no concern about adverse effects on magnetic properties, and they effectively function as elimination points for dislocations caused by deformation. This mechanism of action in this embodiment can be viewed as a special phenomenon in the specific shape of the iron core targeted in this embodiment, and although it has been almost completely overlooked until now, it can be explained in accordance with the insights obtained by the inventors.
[0127] In this embodiment, the frequency of the presence of subgrain boundaries can be determined as follows.
[0128] In this embodiment, the following four angles α, β, γ, and Φ, which are related to the crystal orientation observed in the directional electromagnetic steel plate 1, are used. 3D Furthermore, as will be discussed later, angle α means rotation about the direction Z, the normal to the rolled surface, from the ideal {110} <001> The offset angle (Goss orientation), angle β, means the rotation axis from the ideal {110} with the rolling right-angle direction (plate width direction) C as the axis of rotation. <001> The orientation offset angle, angle γ, means the rotation from the ideal {110} with the rolling direction L as the axis of rotation. <001> The offset angle of orientation.
[0129] Here, the so-called "ideal {110}" <001> "Orientation" does not refer to the crystal orientation of a practical steel sheet {110} <001> Orientation, but rather as an academic crystal orientation {110} <001> orientation.
[0130] Generally, in determining the crystal orientation of recrystallized practical steel sheets, the crystal orientation is defined in a way that does not strictly distinguish between angle differences of approximately ±2.5°. For conventional directional electromagnetic steel sheets, however, the orientation is defined using a geometrically strict {110}... <001> The angular range of approximately ±2.5° centered on the orientation is designated as "{110}". <001> "Orientation". However, in this embodiment, it is also necessary to clearly distinguish angle differences below ±2.5°.
[0131] Therefore, regarding {110} as a geometrically strict crystal orientation <001> In this embodiment, the orientation is specified to avoid the use of {110} in previously known documents, etc. <001> The confusion of orientations is recorded as "ideal {110}". <001> Orientation (ideal Goss orientation)".
[0132] Offset angle α: The crystal orientation observed in the directional electromagnetic steel sheet 1, around the rolling surface normal direction Z, from the ideal {110} <001> The offset angle of orientation.
[0133] Offset angle β: The crystal orientation observed in the directional electromagnetic steel sheet 1, around the rolling right-angle direction C, from the ideal {110} <001> The offset angle of orientation.
[0134] Offset angle γ: The crystal orientation observed in the directional electromagnetic steel sheet 1 around the rolling direction L from the ideal {110} <001> The offset angle of orientation.
[0135] Figure 7 The diagram shows the aforementioned offset angles α, β, and γ.
[0136] Angle Φ 3D When the offset angles of the crystal orientation measured at two adjacent measurement points with a 2mm interval on the rolled surface of the directional electromagnetic steel sheet are expressed as (α1, β1, γ1) and (α2, β2, γ2), respectively, it is through Φ 3D =[(α2-α1) 2 +(β2-β1) 2 +(γ2-γ1) 2 ] 1 / 2 And the angle obtained.
[0137] Sometimes this angle Φ 3D It is recorded as "spatial three-dimensional orientation difference".
[0138] Currently, the crystal orientation of directional electromagnetic steel sheets used in practical manufacturing is determined by the rolling direction and <001> The directional offset angle is controlled to be approximately 5° or less. This control is also applied to the directional electromagnetic steel sheet 1 described in this embodiment. Therefore, when defining the "grain boundary" of the directional electromagnetic steel sheet, the general definition of a grain boundary (large-angle grain boundary), i.e., "a boundary where the orientation difference between adjacent regions is 15° or more," cannot be applied. For example, in conventional directional electromagnetic steel sheets, grain boundaries are revealed by macroscopic corrosion of the steel sheet surface, but the crystal orientation difference between the two sides of the grain boundary is usually around 2 to 3°.
[0139] In this embodiment, as will be described later, it is necessary to strictly define the boundaries between crystals. Therefore, as a specific method for grain boundaries, a visually based method such as macroscopic etching is not adopted.
[0140] In this embodiment, for specific grain boundaries, measurement points are set at 2mm intervals on the rolled surface of the directional electromagnetic steel plate 1, and the crystal orientation is measured at each measurement point. For example, the crystal orientation can be determined by X-ray diffraction (Laué method). The Laué method is a method of analyzing the transmitted or reflected diffraction spots by irradiating the steel plate with an X-ray beam. By analyzing the diffraction spots, the crystal orientation at the irradiated location can be identified. By changing the irradiation position and analyzing the diffraction spots at multiple locations, the crystal orientation distribution at each irradiation location can be determined. The Laué method is suitable for determining the crystal orientation of metal structures with coarse grains.
[0141] The measurement points in this embodiment are as follows: Figure 9 As shown, in the region of the planar portions 4 and 4a adjacent to the curved portion 5, the plates are arranged at equal intervals (2mm intervals) in directions parallel and perpendicular to the boundaries of the curved portion 5 and the planar portions 4 and 4a. In the direction parallel to this boundary, starting from the center of the width of the directional electromagnetic steel plate 1, 20 points are arranged on each side, totaling 41 points. In the direction perpendicular to this boundary, 5 points are arranged starting from a point 1mm away from the boundary. This results in a total of 205 measurement points. By performing measurements on at least 10 steel plates at 205 points, a total of 2050 points are measured. However, since the error in orientation measurement increases when the measurement points are near the ends in the width direction of the steel plate, making it prone to abnormal data, measurement points near the cut ends are avoided during measurement. In other words, when the width of the steel plate is approximately 80mm or less, it can be understood that the number of measurement points in the direction parallel to this boundary can be appropriately reduced. Furthermore, Figure 9 In this text, to facilitate understanding of the location of the measurement points, and for convenience, the size ratios (spacing and grid spacing) of each component are expressed using ratios different from the actual values. That is to say, Figure 9 The grid diagram shown is a conceptual diagram and does not reflect the actual dimensions.
[0142] Here, the size of the measurement area in the direction perpendicular to the boundary of the curved portion 5 and the planar portions 4, 4a is preferably defined as a location at a maximum distance of 9 mm from the boundary. This measurement area is relatively short because the elastic strain occurring in the curved portion 5 only extends into the plastic strain region, i.e., an area several times the size of the curved portion 5. Alternatively, because dislocations only move to at most several times the size of the deformed region, even if subgrain boundaries exist at a distance greater than this, their function as a mitigation of strain caused by subgrain boundaries and an obstacle to dislocation movement is difficult to achieve. Furthermore, the width of the measurement area in the direction parallel to this boundary is approximately 80 mm. This is set considering that in a typical directional electromagnetic steel sheet, it is preferable to measure an area at least covering the total width of one grain, and that the efficiency of the measurement operation decreases if the number of measurement points increases. If sufficient time is spent on the measurement, it is preferable to increase the number of measurement points in the parallel direction, preferably covering the total width of the directional electromagnetic steel sheets stacked to form the wound core.
[0143] Furthermore, when it is difficult to determine the crystal orientation of the planar portions 4 and 4a near the bend 5, a steel plate is cut from the planar portions 4 and 4a in an area at least five times the size of the measurement target area in the aforementioned vertical direction. The measurement points for the crystal orientation of this steel plate are arranged at equal intervals (2 mm intervals) in both the parallel and vertical directions. In the parallel direction, 20 points are arranged on each side of the center of the steel plate's width, totaling 41 points. In the vertical direction, 21 points are arranged, and a total of 861 points are measured on 10 steel plates, for a total of 8610 measurements. In this way, by deriving the average frequency of the subgrain boundaries of the steel plate, which is the raw material for the core, it can be used as a substitute value for the crystal orientation measurement value near the bend. Of course, to derive the average frequency of the subgrain boundaries with high accuracy, it is preferable to increase the number of measurement points in the vertical direction, and it is also preferable to increase the number of measurement points in the parallel direction as described above.
[0144] The above measurements are performed, and for each measurement point, the aforementioned offset angles α, β, and γ are specified. Based on each specified offset angle at each measurement point, it is determined whether a subgrain boundary exists on the line segment connecting two adjacent measurement points. Specifically, in the region of the first plane portion 4 or the second plane portion 4a adjacent to the curved portion 5, multiple measurement points are arranged at 2mm intervals in directions parallel and perpendicular to the boundary of the curved portion 5, i.e., the boundary of the curved portion, to determine whether a subgrain boundary exists on the line segment connecting two adjacent measurement points.
[0145] Furthermore, in this embodiment, the concept of "grain boundary point" used to determine the presence or absence of a grain boundary and the number of grain boundaries between two measurement points can also be defined and specified.
[0146] Specifically, the aforementioned angle Φ at two adjacent measurement points3D 2.0° > Φ 3D The case of ≥0.5° is determined to be the presence of a grain boundary point satisfying the boundary condition BA at the center between the two points, Φ 3D The case of ≥2.0° is determined to be a grain boundary point that satisfies the boundary condition BB at the center between the two points.
[0147] Grain boundaries satisfying boundary condition BA are the subgrain boundaries that this embodiment focuses on. On the other hand, grain boundaries satisfying boundary condition BB are roughly the same as the grain boundaries of conventional secondary recrystallized grains as understood through macroscopic corrosion.
[0148] Grain boundary point determination is performed on each line segment connecting two adjacent points in the aforementioned parallel and perpendicular directions. That is, points adjacent in the inclined direction are not determined. When 41 measurement points are set in the parallel direction and 5 measurement points are set in the perpendicular direction, and 10 steel plates are measured, grain boundary point determination is performed on 3640 locations (that is, a total of 3640 line segments). The total number of locations where grain boundary point determination is performed (the total number of line segments) is set as Nt (3640 in the aforementioned measurements). Between two adjacent points in a direction parallel to the boundary of the aforementioned curved section 5 (the width direction of the directional electromagnetic steel plate 1), the number of grain boundary points satisfying the aforementioned boundary condition BA is set as Nac, and the number of grain boundary points satisfying the aforementioned boundary condition BB is set as Nbc. That is, among line segments in a direction parallel to the boundary of the curved section, the number of line segments where subgrain boundaries can be identified is set as Nac, and the number of line segments where subgrain boundaries cannot be identified is set as Nbc. Furthermore, between two adjacent points in a direction perpendicular to the boundary of the aforementioned curved portion 5 (the rolling direction of the directional electromagnetic steel sheet 1), the number of grain boundary points satisfying the aforementioned boundary condition BA is set as Na1, and the number of grain boundary points satisfying the aforementioned boundary condition BB is set as Nbl. In other words, among the line segments in the direction perpendicular to the boundary of the curved portion, the number of line segments in which subgrain boundaries can be identified is set as Na1, and the number of line segments in which subgrain boundaries cannot be identified is set as Nbl.
[0149] The directional electromagnetic steel plate 1 according to this embodiment has grain boundaries satisfying boundary condition BA at a relatively high frequency compared to grain boundaries satisfying boundary condition BB. This allows dislocations that occur in the bending portion 5 and move towards the planar portions 4, 4a to be effectively eliminated, or elastic strain to be mitigated. As a result, core efficiency can be improved.
[0150] It is important to note that grain boundaries satisfying boundary condition BB, i.e., conventional grain boundaries, also have the effect of dislocation disappearance. In other words, even when grain boundaries satisfying boundary condition BA are completely absent, the effect of dislocation disappearance can still be expected through grain boundaries satisfying boundary condition BB. For example, if the number of grain boundary points satisfying boundary condition BB is increased by refining the grain size, the dislocation disappearance effect is manifested accordingly. However, in this case, there is a concern about the decrease in magnetic properties caused by finer grains. In order to clarify the characteristics of subgrain boundaries that can effectively play a role in dislocation disappearance compared to conventional grain boundaries, this embodiment specifically requires that there be a certain number or more grain boundary points satisfying boundary condition BA.
[0151] In the wound iron core according to this embodiment, the following formula (1) is satisfied in the planar portions 4, 4a near at least one bent portion 5 of the stacked arbitrary directional electromagnetic steel plate 1.
[0152] (Nac+Nal) / Nt≥0.010 (1)
[0153] The numerator on the left side of equation (1) is the sum of grain boundary points where subgrain boundaries can be identified within the measurement area. The definition in equation (1) corresponds to the basic characteristics of the mechanism described above. That is, the left side ((Nac+Nal) / Nt) in equation (1) is an index representing the density of subgrain boundaries per unit area. In the wound core of this embodiment, it is important to ensure that this density is above a certain level in the vicinity of the bend 5. By satisfying equation (1), the subgrain boundaries become obstacles to the movement of dislocations occurring in the bend 5 toward the planes 4 and 4a, thereby demonstrating the effect of the present invention. Preferably, the left side of equation (1) is 0.030 or more, more preferably 0.050 or more. Furthermore, it is of course preferable that equation (1) is satisfied in all planes 4 and 4a adjacent to the bend 5 in the wound core.
[0154] As another embodiment, the following formula (2) is further satisfied in the planar portions 4, 4a near at least one curved portion 5 of the stacked arbitrary directional electromagnetic steel plate 1.
[0155] (Nac+Nal) / (Nbc+Nbl)>0.30 (2)
[0156] This provision specifically corresponds to the characteristic that subgrain boundaries are more likely to act as barriers to dislocation movement than ordinary grain boundaries, and corresponds to one of the preferred embodiments of this invention. By satisfying the above formula (2), the movement of dislocations into the planar region can be sufficiently suppressed. Regarding the left side of formula (2), it is preferably 0.80 or more, more preferably 1.80 or more. Furthermore, it is of course preferable that the above formula (2) is satisfied in all the planar portions 4, 4a adjacent to the bent portion 5 present in the wound core.
[0157] As another embodiment, it is characterized in that, in the planar portions 4, 4a near at least one curved portion 5 of the stacked arbitrary directional electromagnetic steel plate 1, the following formula (3) is further satisfied.
[0158] Nal / Nac≥0.80 (3)
[0159] Taking into account the mechanism described above, this provision particularly corresponds to the following feature: subgrain boundaries that intersect with the direction toward the plane portions 4, 4a (the direction perpendicular to the boundary of the curved portion 5) are more likely to act as obstacles to the movement of dislocations toward the plane portions 4, 4a than subgrain boundaries that exist parallel to the direction toward the plane portions 4, 4a (the direction perpendicular to the boundary of the curved portion 5). By satisfying the above formula (3), the movement of dislocations toward the plane portion region can be sufficiently suppressed. Regarding the left side of formula (3), it is preferably 1.0 or more, more preferably 1.5 or more. Furthermore, it is of course preferable that the above formula (3) is satisfied in all the plane portions 4, 4a adjacent to the curved portion 5 present in the wound core.
[0160] (2) Directional electromagnetic steel sheet
[0161] As described above, in the directional electromagnetic steel plate 1 used in this embodiment, the mother steel plate is in which the grains are highly oriented and clustered in {110}. <001> Oriented steel sheets are steel sheets that have excellent magnetic properties in the rolling direction.
[0162] In this embodiment, the mother steel plate can be a known directional electromagnetic steel plate. Hereinafter, an example of a preferred mother steel plate will be described.
[0163] The chemical composition of the mother steel plate, by mass%, contains 2.0%–6.0% Si, with the remainder consisting of Fe and impurities. This chemical composition is used to control the crystal orientation to aggregate in {110}. <001> The oriented Goss texture ensures good magnetic properties. There are no particular limitations regarding other elements, but in this embodiment, in addition to Si, Fe, and impurities, the following selective elements may also be included. For example, by substituting a portion of Fe, the following elements may be included within the specified range. Representative ranges of these selective elements are described below.
[0164] C:0~0.0050%、
[0165] Mn:0~1.0%、
[0166] S:0~0.0150%、
[0167] Se:0~0.0150%、
[0168] Al:0~0.0650%、
[0169] N:0~0.0050%、
[0170] Cu:0~0.40%、
[0171] Bi:0~0.010%、
[0172] B:0~0.080%、
[0173] P:0~0.50%、
[0174] Ti:0~0.0150%、
[0175] Sn:0~0.10%、
[0176] Sb:0~0.10%、
[0177] Cr:0~0.30%、
[0178] Ni:0~1.0%、
[0179] Nb:0~0.030%、
[0180] V:0~0.030%、
[0181] Mo:0~0.030%、
[0182] Ta:0~0.030%、
[0183] W:0~0.030%.
[0184] Since these selected elements only need to be present according to their purpose, their lower limit value does not need to be limited, and they can be substantially absent. Furthermore, even if these selected elements are present as impurities, it does not impair the effect of this embodiment. Moreover, it is difficult to specify the C content as 0% in practical steel sheets, so the C content can be specified as exceeding 0%. Furthermore, among these selected elements, Nb, V, Mo, Ta, W, and especially Nb, are known to influence the morphology of inhibitors in directional electromagnetic steel sheets, thereby increasing the frequency of subgrain boundaries, and are therefore elements that should be actively used in this embodiment. When the effect of increasing the subgrain boundary frequency is desired, it is preferable to contain at least one selected from Nb, V, Mo, Ta, and W in total of 0.0030 to 0.030% by mass. Furthermore, impurities refer to elements that are unintentionally present, meaning elements that are mixed in from the ore, waste, or manufacturing environment used as raw materials during the industrial manufacture of the mother steel sheet. The upper limit of the total impurity content can be, for example, 5%.
[0185] The chemical composition of the base steel plate can be determined using general analytical methods for steel. For example, the chemical composition of the base steel plate can be determined using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Specifically, for example, a 35mm square test piece can be obtained from the center of the base steel plate after the covering film has been removed, and the composition can be determined using a Shimadzu ICPS-8100 (measuring device) under conditions based on a pre-prepared calibration curve. Furthermore, C and S can be determined using the combustion-infrared absorption method, and N can be determined using the inert gas melting-thermal conductivity method.
[0186] Furthermore, the aforementioned chemical composition refers to the composition of the directional electromagnetic steel plate 1, which serves as the mother steel plate. When the directional electromagnetic steel plate 1, which becomes the test sample, has a primary coating film (glass coating film, intermediate layer), an insulating coating film, etc., formed from oxides or the like on its surface, the chemical composition is determined after removing these films using the method described below.
[0187] For example, as a method for removing the insulating covering film, the directional electromagnetic steel plate with the covering film can be simply immersed in a high-temperature alkaline solution. Specifically, in a sodium hydroxide aqueous solution of NaOH: 30-50% by mass + H₂O: 50-70% by mass, immersion at 80-90°C for 5-10 minutes, followed by washing with water and drying, can remove the insulating covering film from the directional electromagnetic steel plate. Furthermore, the immersion time in the aforementioned sodium hydroxide aqueous solution can be varied according to the thickness of the insulating covering film.
[0188] Furthermore, for example, as a method for removing the intermediate layer, the electromagnetic steel sheet with the insulating cover film removed can be immersed in high-temperature hydrochloric acid. Specifically, in order to remove the intermediate layer to be dissolved, the preferred concentration of hydrochloric acid is investigated in advance. In hydrochloric acid of this concentration, for example, 30-40% by mass hydrochloric acid, immersion at 80-90°C for 1-5 minutes, followed by washing with water and drying, can remove the intermediate layer. Generally, the treatment solutions are used separately to remove each cover film, with an alkaline solution used for removing the insulating cover film and hydrochloric acid used for removing the intermediate layer.
[0189] (3) Manufacturing method of directional electromagnetic steel sheet
[0190] The manufacturing method of the mother steel plate, i.e., the directional electromagnetic steel plate 1, is not particularly limited. By strictly controlling the final annealing process as described later, grain boundaries (grain boundaries that divide secondary recrystallized grains) that satisfy boundary condition BA but do not satisfy boundary condition BB can be intentionally implanted. By using such a directional electromagnetic steel plate with grain boundaries that satisfy boundary condition BA but do not satisfy boundary condition BB (grain boundaries that divide secondary recrystallized grains) to manufacture the wound iron core, a wound iron core that can suppress the deterioration of iron core efficiency can be obtained. In addition, the grain boundaries that satisfy boundary condition BA but do not satisfy boundary condition BB (grain boundaries that divide secondary recrystallized grains) can fully achieve the effect of mitigating the strain during iron core processing. Therefore, during the baking annealing of the insulating coating, it is preferable to set the cooling rate from 800°C to 500°C to 60°C / second or less, and more preferably to 50°C / second or less. In addition, there is no particular limitation on the lower limit of this cooling rate, but considering the deterioration of productivity and the cooling capacity of the furnace body, as well as the fact that the length of the cooling zone is not excessively extended, it is practically preferable to be 10°C / second or more, and more preferably 20°C / second or more.
[0191] Specifically, in the final annealing process, when the total content of Nb, V, Mo, Ta, and W in the slab's chemical composition is 0.0030 to 0.030%, it is preferable to control the pH2O / pH2 ratio during the heating process to be 0.030 to 5.0 at 700 to 800°C, 0.010 to 0.20 at 900 to 950°C, 0.005 to 0.10 at 950 to 1000°C, or 0.0010 to 0.050 at 1000 to 1050°C. Further preferably, it is preferable to control the holding time at 950 to 1000°C to be 150 minutes or more, or the holding time at 1000 to 1050°C to be 150 minutes or more.
[0192] In addition, it is preferable to set the holding time at 1050–1100°C to 300 minutes or more.
[0193] On the other hand, when the total content of Nb, V, Mo, Ta, and W in the chemical composition of the above-mentioned slab is not 0.0030 to 0.030%, it is preferable to control the pH2O / pH2 ratio during the heating process to be 0.030 to 5.0 at 700 to 800°C, 0.010 to 0.20 at 900 to 950°C, 0.0050 to 0.10 at 950 to 1000°C, or 0.0010 to 0.050 at 1000 to 1050°C. In this case, it is further preferable to control the holding time at 950 to 1000°C to be 300 minutes or more, or the holding time at 1000 to 1050°C to be 300 minutes or more.
[0194] In addition, it is preferable to set the holding time at 1050–1100°C to 300 minutes or more.
[0195] Furthermore, it is more preferable to generate secondary recrystallization by applying a temperature gradient exceeding 0.5°C / cm to the boundary between the primary recrystallization region and the secondary recrystallization region in the steel sheet during the heating process of the final annealing step. For example, it is preferable to apply the aforementioned temperature gradient to the steel sheet during the growth of secondary recrystallized grains within a temperature range of 800°C to 1150°C during the heating process of the final annealing. Furthermore, it is preferable that the direction in which the aforementioned temperature gradient is applied is the rolling right-angle direction C.
[0196] The aforementioned PH2O / PH2 is called oxygen potential, which is the ratio of the partial pressure of water vapor PH2O to the partial pressure of hydrogen PH2 in the atmosphere.
[0197] As a preferred specific example of the manufacturing method, the following method can be cited, in which a slab having the above-mentioned chemical composition of the parent steel plate, wherein C is specified as 0.04 to 0.1% by mass, is heated to above 1000°C and hot-rolled, then hot-rolled annealing is performed as needed. Next, a cold-rolled steel sheet is formed by one or more cold rolling processes, including intermediate annealing. This cold-rolled steel sheet is then decarburized and annealed, for example, in a wet hydrogen-inert gas atmosphere to 700 to 900°C. Further nitriding annealing is performed as needed. After applying an annealing separating agent, a final annealing is performed at approximately 1000°C, and an insulating covering film is formed at approximately 900°C. Finally, coating for adjusting the coefficients of dynamic and static friction can also be implemented.
[0198] Furthermore, even steel sheets that have undergone a process known as "magnetic domain control" during the steel sheet manufacturing process can generally enjoy the effects of this embodiment.
[0199] The characteristic of the directional electromagnetic steel plate 1 used in this embodiment, namely the subgrain boundaries, can be adjusted, for example, by the processing atmosphere and residence time of each temperature zone of the final annealing, as disclosed in Patent Document 7. There are no particular limitations on the method; any known method can be appropriately employed. By thus pre-increasing the subgrain boundary formation frequency of the entire steel plate, it is expected that the aforementioned conditions will be met in the wound core even when the bend 5 is formed at any position during the manufacturing of the wound core. Alternatively, in order to manufacture a wound core with more subgrain boundaries near the bend 5, it is also effective to control the position of the bent steel plate by placing the portion with a higher subgrain boundary frequency near the bend 5. In this method, when manufacturing the steel plate, it is sufficient to manufacture a steel plate with locally varied secondary recrystallized grain growth by using known methods such as locally altering the primary recrystallization structure, nitriding conditions, and the state of the annealing separating agent coating, and selectively perform bending processing on the portions with increased subgrain boundary frequencies.
[0200] 3. Manufacturing method of wound iron core
[0201] The method for manufacturing the wound iron core according to this embodiment is not particularly limited as long as it can manufacture the wound iron core according to this embodiment. For example, the method based on a known wound iron core described in patent documents 9-11 in the background art can be applied. In particular, it can be said that the method using the UNICORE (https: / / www.aemcores.com.au / technology / unicore / ) manufacturing apparatus of AEM UNICORE Corporation is most suitable.
[0202] Alternatively, heat treatment can be performed as needed using known methods. Furthermore, the resulting wound core body 10 can be used directly as a wound core, or, as needed, the stacked directional electromagnetic steel plates 1 can be fixed with known fasteners such as cable ties to form a wound core.
[0203] This embodiment is not limited to the above-described embodiment. The above-described embodiment is an example, and any structure having substantially the same technical concept as that described in the claims of this invention, and achieving the same effect, is included within the technical scope of this invention.
[0204] Example
[0205] The technical content of the present invention will be further described below while listing embodiments. The conditions in the embodiments shown below are examples of conditions adopted to confirm the feasibility and effect of the present invention, and the present invention is not limited to these examples. In addition, various conditions can be adopted as long as they do not depart from the spirit of the present invention and achieve the purpose of the present invention.
[0206] (Directional electromagnetic steel sheet)
[0207] Using slabs with the composition shown in Table 1 (mass %, the remainder excluding the indicated portion is Fe) as raw materials, directional electromagnetic steel sheets (product sheets) with the composition shown in Table 2 (mass %, the remainder excluding the indicated portion is Fe) and sheet thickness t (μm) are manufactured. Here, the final annealing conditions are those described in Patent Document 7, etc., to change the subgrain boundary frequency near the bending portion. "-" in Tables 1 and 2 indicates elements for which conscious content control and manufacturing were not performed, and for which content determination was not carried out.
[0208]
[0209]
[0210] (Evaluation Method)
[0211] (1) Subgrain boundary frequency
[0212] For steel plates (steel grades A1 to D1) manufactured using the above method, crystal orientation measurement points totaling 205 points were arranged at 2mm intervals in an 8mm × 80mm area near the bend, as described above, and crystal orientation measurement was performed. This measurement was also performed on 10 other steel plates. Based on the results of the total 2050 measurements, grain boundary points between adjacent measurement points were determined at 3640 locations, and Nac, Naal, Nbc, Nbl, etc., were calculated.
[0213] (2) Magnetic properties of directional electromagnetic steel sheets
[0214] The magnetic properties of the directional electromagnetic steel plate 1 were measured based on the Single Sheet Tester (SST) method specified in JIS C 2556:2015.
[0215] As a magnetic property, the magnetic flux density B8(T) in the rolling direction of the steel plate when excited at 800 A / m and the iron loss value of the steel plate when the excitation magnetic flux density is 1.7 T and the frequency is 50 Hz were measured.
[0216] (3) Efficiency of the iron core
[0217] Using various steel plates as raw materials, manufacture products with the features shown in Table 3 and... Figure 8The cores No. a to c are shown in the diagram. Furthermore, L1, parallel to the X-axis, is the distance between the innermost parallel directional electromagnetic plates 1 located on the innermost periphery of the wound core in the plan cross section including the center CL (distance between inner side planar portions). L1′, parallel to the X-axis, is the length of the first planar portion 4 of the innermost directional electromagnetic plate 1 (length of the inner side planar portion). L2, parallel to the Z-axis, is the distance between the innermost parallel directional electromagnetic plates 1 located on the innermost periphery of the wound core in the longitudinal section including the center CL (distance between inner side planar portions). L2′, parallel to the Z-axis, is the length of the first planar portion 4 of the innermost directional electromagnetic plate 1 (length of the inner side planar portion). L3, parallel to the X-axis, is the stacking thickness of the wound core in the plan cross section including the center CL (thickness in the stacking direction). L4, parallel to the X-axis, is the width of the stacked steel plates of the wound core in the plan cross section including the center CL. L5 is the distance between the innermost planar portions (the distance between the curved portions) of the wound iron core, which are arranged in a way that is adjacent to each other and simultaneously form right angles. In other words, L5 is the length of the shortest planar portion 4a among the planar portions 4 and 4a of the innermost circumference of the directional electromagnetic steel plate 1. r is the radius of curvature of the curved portion 5 on the inner side of the wound iron core, and Φ is the bending angle of the curved portion 5 of the wound iron core.
[0218] By measuring the iron loss of the obtained wound core, the core efficiency, commonly referred to as the building factor (BF), which is calculated as the ratio of these iron losses, was determined. Here, BF is the value obtained by dividing the iron loss of the wound core by the iron loss of the raw material for the wound core, namely the directional electromagnetic steel sheet. The smaller the BF, the lower the iron loss of the wound core relative to the raw material steel sheet. Furthermore, in this embodiment, a BF of 1.12 or less is evaluated as being able to suppress the deterioration of iron loss efficiency.
[0219] Table 3
[0220]
[0221] (Example 1: No. 1-6)
[0222] Using steel grade A1, steel plates A1-(1~6) with altered subgrain boundary frequencies were manufactured according to the final annealing atmosphere and thermal cycling conditions. The wound core of core No.a was then manufactured, and the core efficiency was evaluated.
[0223] (Example 2: No.7-12)
[0224] Using steel grade B1, the heating rate during decarburization annealing was set to 50–400 °C / s. Steel plates B1-(1–6) with partially modified grain size were manufactured, and a wound core of core No.b was produced. The core efficiency was evaluated.
[0225] (Example 3: No. 13-25)
[0226] Using steel grade C1, steel plates C1-(1~9) with significantly altered subgrain boundary frequencies were manufactured under the final annealing atmosphere and temperature gradient conditions. A wound core No.b with altered bending shape (inner side curvature radius r) was manufactured in C1-8, and the core efficiency was evaluated (mainly evaluating the difference in the influence of subgrain boundary frequency and bending morphology).
[0227] (Example 4: No. 26-36)
[0228] Using steel grade D1, steel plates D1-(1~11) with significantly altered subgrain boundary frequencies were manufactured under the final annealing atmosphere and temperature gradient conditions. Cores of core No.c were then manufactured, and core efficiency was evaluated (mainly evaluating the differences in the influence of subgrain boundary frequency and bending morphology).
[0229] (Example 5: No. 37-52)
[0230] Using steel grades E1 to T1, steel plates with significantly altered subgrain boundary frequencies were manufactured according to the final annealing atmosphere, holding time, and temperature gradient conditions. Any one of the cores No. a to c was then manufactured, and the core efficiency was evaluated.
[0231] In addition, Table 4 shows the core efficiency evaluation results of Examples 1 to 3. Furthermore, in the "judgment" of equations (1) to (3) in Table 4, the symbol "〇" means that the equation is satisfied, and the symbol "×" means that the equation is not satisfied.
[0232]
[0233]
[0234]
[0235]
[0236]
[0237]
[0238]
[0239]
[0240]
[0241] The above results show that the wound core of the present invention has the characteristic of low iron loss because at least one of two or more bends 5 in at least one corner 3 satisfies the above formula (1).
[0242] Industrial availability
[0243] According to the present invention, in a wound iron core formed by stacking layers of bent steel plates, efficiency degradation caused by carelessness can be effectively suppressed.
[0244] Symbol explanation:
[0245] 1 Directional Electromagnetic Steel Sheet
[0246] 2-layer structure
[0247] 3 corners
[0248] 4. Planar section
[0249] 5. Bending section
[0250] 6 joints
[0251] 10-winding iron core body
Claims
1. A wound iron core, comprising a wound iron core body that is generally rectangular in shape when viewed from the side, characterized in that: In the main body of the wound iron core, the first flat portion and the corner portion are continuously alternately arranged in the length direction, including a portion formed by stacking directional electromagnetic steel plates in the thickness direction by two adjacent first flat portions sandwiching each corner portion at an angle of 90°, and having a stacked structure that is roughly rectangular in shape when viewed from the side. Each corner portion, in a side view of the directional electromagnetic steel plate, has two or more curved portions with a curved shape, and a second flat portion is provided between adjacent curved portions, and the total curvature angle of each curved portion in a corner portion is 90°. The inner side curvature radius r of the curved portion in the side view is more than 1 mm and less than 5 mm; In the directional electromagnetic steel plate, Its chemical composition, expressed as a percentage by mass, contains: Si: 2.0–7.0% The remaining portion includes Fe and impurities. It has a texture oriented towards the Goss orientation, and In one or more of the first planar portion and the second planar portion adjacent to at least one of the curved portions, the frequency of the presence of subgrain boundaries in the region within 9 mm of the boundary between the curved portion and the planar portion along a direction perpendicular to the boundary satisfies the following equation (1). (Nac+Nal) / Nt≥0.010 (1) Here, Nt in equation (1) is: the total number of line segments connecting two adjacent measurement points in the parallel and vertical directions of the boundary of the curved portion when multiple measurement points are arranged at 2mm intervals in the region of the first plane portion or the second plane portion adjacent to the curved portion. In Equation (1), Nac is the number of line segments in the direction parallel to the boundary of the curved portion that can identify subgrain boundaries, and Nal in Equation (1) is the number of line segments in the direction perpendicular to the boundary of the curved portion that can identify subgrain boundaries.
2. The wound iron core according to claim 1, characterized in that: In one or more of the first planar portion and the second planar portion adjacent to at least one of the curved portions, the following equation (2) is satisfied. (Nac+Nal) / (Nbc+Nbl)>0.30 (2) Here, Nbc in equation (2) is the number of line segments in the direction parallel to the boundary of the curved portion that can identify grain boundaries other than the subgrain boundary, and Nbl in equation (2) is the number of line segments in the direction perpendicular to the boundary of the curved portion that can identify grain boundaries other than the subgrain boundary.
3. The wound iron core according to claim 1 or 2, characterized in that: In one or more of the first planar portion and the second planar portion adjacent to at least one of the curved portions, the following equation (3) is satisfied. Nal / Nac≥0.80 (3).
4. The wound iron core according to claim 1 or 2, characterized in that: The chemical composition of the directional electromagnetic steel sheet, by mass%, contains: Si: 2.0–7.0% Nb: 0~0.030%, V:0~0.030%、 Mo: 0–0.030% Ta: 0~0.030%, W:0~0.030%、 C:0~0.0050%、 Mn: 0~1.0%, S:0~0.0150%、 Se: 0~0.0150%, Al:0~0.0650%、 N:0~0.0050%、 Cu: 0–0.40% Bi: 0~0.010%, B:0~0.080%、 P:0~0.50%、 Ti: 0~0.0150%, Sn: 0~0.10%, Sb: 0~0.10%, Cr: 0–0.30%, and Ni: 0~1.0%, The remainder includes Fe and impurities.
5. The wound iron core according to claim 3, characterized in that: The chemical composition of the directional electromagnetic steel sheet, by mass%, contains: Si: 2.0–7.0% Nb: 0~0.030%, V:0~0.030%、 Mo: 0–0.030% Ta: 0~0.030%, W:0~0.030%、 C:0~0.0050%、 Mn: 0~1.0%, S:0~0.0150%、 Se: 0~0.0150%, Al:0~0.0650%、 N:0~0.0050%、 Cu: 0–0.40% Bi: 0~0.010%, B:0~0.080%、 P:0~0.50%、 Ti: 0~0.0150%, Sn: 0~0.10%, Sb: 0~0.10%, Cr: 0–0.30%, and Ni: 0~1.0%, The remainder includes Fe and impurities.
6. The wound iron core according to claim 1 or 2, characterized in that: The chemical composition of the directional electromagnetic steel sheet contains a total of 0.0030 to 0.030% by mass of at least one of Nb, V, Mo, Ta and W.
7. The wound iron core according to claim 3, characterized in that: The chemical composition of the directional electromagnetic steel sheet contains a total of 0.0030 to 0.030% by mass of at least one of Nb, V, Mo, Ta and W.
8. The wound iron core according to claim 4, characterized in that: The chemical composition of the directional electromagnetic steel sheet contains a total of 0.0030 to 0.030% by mass of at least one of Nb, V, Mo, Ta and W.
9. The wound iron core according to claim 5, characterized in that: The chemical composition of the directional electromagnetic steel sheet contains a total of 0.0030 to 0.030% by mass of at least one of Nb, V, Mo, Ta and W.
Citation Information
Patent Citations
Detection system for floppy disc interchange
JP1987024468A
Grain oriented silicon steel sheet excellent in magnetic property, and its manufacturing method
JP2001192785A
Grain oriented silicon steel sheet excellent in high frequency magnetic property and its producing method
JP2001303214A
Grain oriented silicon steel sheet having no forsterite film, and excellent in adhesion to insulation film, and production method therefor
JP2004143532A