Preparation and application of iron-doped molybdenum oxide photocatalyst
The iron-doped molybdenum oxide catalyst is prepared by a hydrothermal method, which solves the problem of insufficient catalytic activity of pure molybdenum oxide, significantly improves the efficiency and activity of photocatalytic ammonia synthesis, and simplifies the preparation process.
Patent Information
- Application Number
- CN202211454827.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-11-21
AI Technical Summary
Pure molybdenum oxide (MoO2) has insufficient catalytic activity and is difficult to meet the demand for photocatalytic ammonia synthesis.
Iron-doped molybdenum oxide (Fe-MoO2) was prepared by hydrothermal method, CTAB and HNO3 were used to adjust the pH of the solution, and then dropped into a high-pressure reactor drop by drop for hydrothermal reaction to prepare a Fe-MoO2 catalyst with efficient photocatalytic performance.
It achieves more efficient photocatalytic ammonia synthesis performance than pure molybdenum oxide catalysts, increases catalytic active sites, simplifies the preparation process, and avoids the need for high temperature and high pressure.
Smart Images

Figure CN116440911B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photocatalytic ammonia synthesis, and in particular to the preparation of iron-doped molybdenum oxide and its application as a catalyst in photocatalytic ammonia synthesis. Background Art
[0002] With the rapid development of industrialization and modernization, human beings are facing more and more energy and environmental problems. Inspired by photosynthesis in nature, people have developed semiconductor photocatalytic technology, which uses the inexhaustible solar energy in nature to convert into chemical energy. The electrons and holes excited by semiconductor photocatalysts under light can participate in redox reactions and are used for the removal of liquid or gas pollutants, CO2 reduction to chemical fuels, water decomposition to produce hydrogen and oxygen, and N2 fixation.
[0003] As a cheap transition metal oxide and common metal oxide, MoO2 is widely used in lithium-ion batteries and electrochemical supercapacitors. Unlike other metal oxides, MoO2 with a distorted rutile structure exhibits many special properties, such as good chemical resistance, high melting point, excellent chemical stability and metallic conductivity. The unique metallic conductivity of MoO2 is mainly attributed to its relatively high density of states of 4d and 5s free electrons, which are located on Mo in the valence band energy region. According to the first principles reported, the metallic properties of MoO2 are much stronger than the semiconductor properties, and the large number of free electrons gives MoO2 a localized surface plasmon resonance effect. At the same time, the presence of free electrons is believed to increase the catalytic activity of the catalyst.
[0004] However, the catalytic activity of pure MoO2 is far from satisfactory. In general, metal ion modification and defect engineering can well improve the catalytic activity of MoO2. Metal ion modification mainly includes metal ion loading and metal ion doping. The N≡N triple bond is activated by coordinating transition metal complexes (metal = Fe, Mo, Ru and Co, etc.) with N2, thereby reducing the activated N2 to NH3 under mild conditions.
[0005] This patent uses iron-doped molybdenum oxide to successfully prepare iron-doped molybdenum oxide through a hydrothermal method, and uses it as a photocatalyst for the synthesis of ammonia. Summary of the invention
[0006] The present invention aims to provide a preparation method of an iron-doped molybdenum oxide (denoted as Fe-MoO2) photocatalytic material and its application in synthesizing ammonia.
[0007] The technical solution of the present invention is as follows:
[0008] The invention provides an iron-doped molybdenum oxide material, which is applied to photocatalytic synthesis of ammonia.
[0009] The present invention provides an iron-doped molybdenum oxide for photocatalytic synthesis of ammonia, wherein the iron-doped molybdenum oxide is prepared according to the following method:
[0010] (1) Dispersing ammonium molybdate tetrahydrate in distilled water, referred to as solution A;
[0011] (2) dispersing CTAB (cetyltrimethylammonium bromide) in ethanol, referred to as solution B;
[0012] (3) Then add solution B dropwise into solution A and stir at room temperature;
[0013] (4) Adjust the pH of the solution to 1.5-1.6 with HNO3, record it as solution C, and stir at room temperature;
[0014] (5) Dissolve ferric chloride hexahydrate in water and add dropwise into solution C while stirring at room temperature;
[0015] (6) pouring the solution into a high pressure reactor and subjecting it to a hydrothermal reaction at 170-190° C.;
[0016] (7) After the reaction is completed, the reactor is cooled to room temperature;
[0017] (8) Wash with ethanol and distilled water three times respectively, and dry at 50-60°C.
[0018] In some embodiments, the iron-doped molybdenum oxide is prepared according to the following method:
[0019] (1) Disperse 1.4-1.5 parts of ammonium molybdate tetrahydrate in distilled water, referred to as solution A;
[0020] (2) Disperse 0.14-0.15 parts of CTAB (cetyltrimethylammonium bromide) in ethanol, referred to as solution B;
[0021] (3) then drip solution B into solution A dropwise at a rate of 4-6 mL / min and stir at room temperature for 10-20 min;
[0022] (4) Adjust the pH of the solution to 1.5-1.6 with HNO3, record it as solution C, and stir it at room temperature for 20-30 minutes;
[0023] (5) dissolving ferric chloride hexahydrate in water, dripping it into solution C dropwise at a rate of 2-5 mL / min, and stirring at room temperature for 30-60 min;
[0024] (6) Pour the solution into a high pressure reactor and hydroheat at 170-190°C for 24-48h;
[0025] (7) After the reaction is completed, the reactor is cooled to room temperature;
[0026] (8) Wash with ethanol and distilled water three times respectively, and dry at 50-60°C.
[0027] The present invention further uses the aforementioned iron-doped molybdenum oxide as a photocatalytic material for synthesizing ammonia.
[0028] In some embodiments, the application includes the following steps: dispersing 10-100 mg of iron-doped molybdenum oxide in water, irradiating under a xenon lamp for 0.5-2 hours, and stirring to synthesize ammonia. Specifically, 10 mg of Fe-MoO2 and 80-100 mL / min N2 are passed into 40 mL of H2O, and dark treatment is performed after 30 minutes to achieve adsorption-desorption equilibrium between the catalyst and N2. Then turn on the simulated light source and conduct a photocatalytic ammonia synthesis experiment. After 1 hour, take 2 mL of solution from the quartz tube, add 2 mL of reagent A, 1 mL of reagent B and 0.2 mL of reagent C to measure its absorbance. Figure 3 It can be seen that Fe-MoO2 exhibits efficient photocatalytic ammonia synthesis performance compared with simple MoO2.
[0029] The present invention has the following beneficial effects:
[0030] (1) The preparation method is simple, does not require a high temperature process above 200°C, and does not involve co-doping with other elements;
[0031] (2) The constructed loaded catalyst has an increased number of active sites compared to the pure catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is the XRD pattern of MoO2 of Example 1;
[0033] Figure 2 is the XRD pattern of Fe-MoO2 of Example 2;
[0034] Figure 3 This is the photocatalytic ammonia synthesis activity spectrum of Example 3.
[0035] Figure 4 NH4 in Example 4 + Standard curve graph. DETAILED DESCRIPTION
[0036] The present invention is further described below with reference to specific embodiments, but the protection scope of the present invention is not limited thereto.
[0037] Example 1: Preparation method of molybdenum oxide photocatalyst:
[0038] (1) Disperse 1.5 g of ammonium molybdate tetrahydrate in 40 mL of distilled water, referred to as solution A.
[0039] (2) Disperse 0.15 g of CTAB (cetyltrimethylammonium bromide) in 5 mL of ethanol, referred to as solution B.
[0040] (3) Solution B was then added dropwise into solution A at a rate of 6 mL / min and stirred at room temperature for 10 min.
[0041] (4) Adjust the pH of the solution to 1.5 with 1 M HNO3, record it as solution C, and stir it at room temperature for 20 min.
[0042] (5) The solution was poured into a 100 mL Teflon stainless steel autoclave and hydroheated at 170-190 °C for 48 h.
[0043] (6) After the reaction is completed, the reactor is cooled to room temperature.
[0044] (7) Wash with ethanol and distilled water three times respectively, and dry at 50-60°C to obtain MoO2, whose XRD pattern is as follows Figure 1 shown.
[0045] Example 2: Preparation method of iron-doped molybdenum oxide photocatalyst:
[0046] (1) Disperse 1.5 g of ammonium molybdate tetrahydrate in 50 mL of distilled water, referred to as solution A.
[0047] (2) Disperse 0.15 g of CTAB (cetyltrimethylammonium bromide) in 5 mL of ethanol, referred to as solution B.
[0048] (3) Solution B was then added dropwise into solution A at a rate of 6 mL / min and stirred at room temperature for 10-20 min.
[0049] (4) Adjust the pH of the solution to 1.5 with 1 M HNO3, record it as solution C, and stir it at room temperature for 20 min.
[0050] (5) Dissolve ferric chloride hexahydrate in water and add the solution C dropwise at a rate of 2 mL / min. Stir at room temperature for 30 min.
[0051] (6) The solution was poured into a 100 mL Teflon stainless steel autoclave and hydroheated at 180 °C for 48 h.
[0052] (7) After the reaction is completed, the reactor is cooled to room temperature.
[0053] (8) Wash with ethanol and distilled water three times respectively, and dry at 50-60°C to obtain Fe-MoO2, whose XRD pattern is shown in the figure Figure 2 shown.
[0054] Example 3: Photocatalytic experiment
[0055] The simulated sunlight catalytic synthesis of ammonia was used as a model reaction. The absorbance at 655nm was measured by UV-visible spectrophotometer to determine the amount of ammonia generated, so as to evaluate the photocatalytic performance of the material. A 300W xenon lamp (200<λ<800nm) was used as a simulated visible light source in the experiment. 10mg of the catalyst was added to 40mL of water, ultrasonicated for 10min to disperse evenly, and added to a double-layer reaction tube. Subsequently, dark treatment was carried out under magnetic stirring for 30min to achieve adsorption-desorption equilibrium between the catalyst and N2. Then the simulated light source was turned on to conduct a photocatalytic synthesis of ammonia experiment. After 1h of reaction, 2mL of solution was taken from the quartz tube, filtered through a 0.22μm organic filter membrane, and 2mL of reagent A, 1mL of reagent B and 0.2mL of reagent C were added. Wait for 2h to measure its absorbance at 655. According to the standard curve, it was converted to the concentration C (μmol / g / h) of ammonia.
[0056] Figure 3 The illustrated photocatalytic ammonia synthesis activity spectrum reflects that the activity of the iron-doped molybdenum oxide photocatalyst provided in Example 2 is significantly greater than that of the molybdenum oxide photocatalyst provided in Example 1, indicating that the iron doping better improves the light absorption performance of the molybdenum oxide material, thereby greatly improving its activity in the photocatalytic ammonia synthesis reaction.
[0057] Example 4: Preparation of standard curve
[0058] (1) Weigh 1.0 g of NH4Cl and place it in a forced air drying oven at 105°C for 2 h.
[0059] (2) Take the dried NH4Cl prepared above and prepare a 4 μg / mL ammonia standard solution.
[0060] (3) Use a 1000 μL pipette to take 0, 50, 100, 150, 200, 250, 400, 750, 1250 and 2000 μL of NH4 + The standard solutions were added into 5 mL colorimetric tubes and then diluted to 2 mL.
[0061] (4) Finally, add 2 mL of reagent A, 1 mL of reagent B and 0.2 mL of reagent C to the above series of solutions, shake well and let stand for 2 h, then detect the absorbance at λ = 655 nm and perform linear fitting to obtain the standard curve. Figure 4 shown.
[0062] Figure 4 It shows that NH4 + The absorbance is at λ=655nm, and NH4 + The standard curve of absorbance A-concentration C can be used to calculate NH4 based on the absorbance.+ concentration.
Claims
1. An application of an iron-doped MoO2 photocatalyst as a photocatalytic material for synthesizing ammonia, characterized in that: The iron-doped MoO2 photocatalyst is prepared according to the following method: (1) Dispersing ammonium molybdate tetrahydrate in distilled water, referred to as solution A; (2) Dispersing CTAB in ethanol, referred to as solution B; (3) Then add solution B dropwise into solution A and stir at room temperature; (4) Adjust the pH of the solution to 1.5-1.6 with HNO3, record it as solution C, and stir at room temperature; (5) Dissolve ferric chloride hexahydrate in water and add dropwise into solution C while stirring at room temperature; (6) pouring the solution into a high pressure reactor and performing a hydrothermal reaction at 170-190°C; (7) After the reaction is completed, the reactor is cooled to room temperature; (8) Wash with ethanol and distilled water three times respectively, and dry at 50-60°C.
2. The use according to claim 1, characterized in that The iron-doped MoO2 is prepared according to the following method: (1) Disperse 1.4-1.5 parts of ammonium molybdate tetrahydrate in distilled water, referred to as solution A; (2) Disperse 0.14-0.15 parts of CTAB in ethanol, referred to as solution B; (3) Then, solution B was added dropwise into solution A at a rate of 4-6 mL / min and stirred at room temperature for 10-20 min; (4) Adjust the pH of the solution to 1.5-1.6 with HNO3, record it as solution C, and stir it at room temperature for 20-30 minutes; (5) dissolving ferric chloride hexahydrate in water, dripping it into solution C dropwise at a rate of 2-5 mL / min, and stirring at room temperature for 30-60 min; (6) Pour the solution into a high pressure reactor and hydroheat at 170-190 °C for 24-48 h; (7) After the reaction is completed, the reactor is cooled to room temperature; (8) Wash with ethanol and distilled water three times respectively, and dry at 50-60°C.
3. The use according to claim 1, characterized in that: Disperse 10 to 100 mg of iron-doped MoO2 in water, pass N2 into the water, irradiate under a xenon lamp for 0.5 to 2 h, and stir to synthesize ammonia.