A hydrogenation catalyst grading method and its application
By cascading the acid amount and aluminum ion content in the alumina carrier, the catalyst microstructure is optimized, which solves the problem of long-term operation due to impurities in inferior raw materials, improves the utilization rate and stability of the catalyst, and enhances the catalytic performance.
Patent Information
- Application Number
- CN202210012023.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-01-06
AI Technical Summary
The existing heavy oil hydrogenation catalyst grading method cannot effectively solve the problem of impurities in inferior raw materials that make it difficult to operate for a long period of time, resulting in reduced catalyst activity and low utilization.
A multi-stage hydrogenation catalyst grading method is adopted, using acids of different strengths and coordinated aluminum ions in the alumina carrier to perform cascade design. By adjusting the acid amount and aluminum ion content, the microstructure of the catalyst is optimized to match the molecular structure of the reactants to achieve Proper distribution of impurities and simultaneous deactivation of catalysts.
It improves the utilization rate of the catalyst and the long-term operation stability of the device, enhances the catalytic performance, effectively suppresses the deactivation of the catalyst, and improves the removal efficiency of impurities.
Smart Images

Figure CN116440916B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a grading method for hydrogenation catalyst and application thereof, in particular to a grading method for heavy oil hydrogenation catalyst for long-term operation of inferior raw materials and application thereof. Background Art
[0002] During the heavy oil hydrogenation process, as the raw materials become heavier and inferior, the content of metal impurities and inorganic salts such as Fe, Si, Na, Ca in the raw materials continues to increase. These metals mainly exist in the form of colloids and asphaltene. Secondly, the heavy inferior raw materials have low saturated hydrocarbon content, high aromatic hydrocarbon content, and high colloid content, especially high heavy aromatic hydrocarbon content. These heavy raw materials have complex molecular structures, large steric hindrance, and impurities are easier to remove; with the hydrogenation and hydrogenolysis reactions, the reactant molecules gradually open the ring and break the chain, the molecular structure is gradually simplified, the steric hindrance is small, and impurities are more difficult to remove. At present, the grading method of heavy oil hydrogenation catalyst is often studied from the surface level, that is, the catalyst particle size, pore size and activity transition, and it is not considered from the actual reactant molecular structure level and catalyst microstructure. As the reaction proceeds, the reactant molecular structure and catalyst microstructure cannot match well, which limits the depth of the hydrogenation reaction.
[0003] CN103773437A discloses a grading method for a hydrodesulfurization catalyst, the method comprising: a hydrogenation reactor includes at least two catalyst beds, in accordance with the order of contact with the reaction material, the upstream bed is a low-pile ratio catalyst bed, the downstream catalyst bed has a higher pile ratio than the adjacent upstream catalyst bed; each catalyst bed is graded and loaded with two or more catalysts of different diameters. These physical mixtures have a smaller void ratio and a larger loading pile ratio than their single diameter catalysts, which improves the hydrodesulfurization performance of the entire reaction system, but it is difficult to achieve long-term stable operation for processing inferior raw materials with high solid impurity content. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a grading method for hydrogenation catalysts to solve the problem of long-term operation of inferior raw materials, to effectively optimize the activity grading of the overall catalyst, to achieve a reasonable distribution of impurities in the entire system, and thus to achieve the purpose of synchronous deactivation of the entire catalyst system as much as possible, so as to improve the utilization rate of the catalyst and achieve long-term operation of the device.
[0005] To achieve the above object, the present invention provides a hydrogenation catalyst grading method, comprising a grading system composed of n-level hydrogenation catalysts, wherein n ≥ 3, preferably n is 3 or 4, and any level of hydrogenation catalyst comprises an alumina carrier, and the surface of the alumina carrier contains three acids of different strengths: weak acid C R , medium strong acid C Z and strong acid CQ The alumina carrier contains three types of aluminum ions: three-coordinate aluminum ions Al 3+ Ⅲ , four-coordinated aluminum ion Al 3+ IV and pentacoordinated aluminum ion Al 3+ Ⅴ The n-stage hydrogenation catalyst grading satisfies the following conditions: along the flow direction of the liquid phase reactants, based on the total amount of the three acids in the alumina carrier, the acidity of the strong acid ψ Q Increase step by step, the increment is 1×10 4 ~9×10 4 mmol / m 2 , preferably 1×10 4 ~7×10 4 mmol / m 2 ; Based on the total amount of three ligands of aluminum in the alumina carrier, the content of tri-coordinated aluminum ions The increase is gradual, with the increment ranging from 1 to 10 percentage points.
[0006] Furthermore, along the flow direction of the liquid phase reactants, based on the total amount of the three acids in the alumina carrier, the acid amount of the weak acid ψ R Decrease gradually, with a decreasing amplitude of 1×10 4 ~20×10 4 mmol / m 2 , preferably 1×10 4 ~10×10 4 mmol / m 2 .
[0007] Furthermore, along the flow direction of the liquid phase reactants, based on the total amount of the three acids in the alumina carrier, the acid amount of the medium-strong acid ψ Z There are no specific requirements and it can be increased, decreased or unchanged.
[0008] Furthermore, in the alumina support of any stage hydrogenation catalyst, the acidity of the weak acid ψ R is 10×10 4 ~30×10 4 mmol / m 2 , the acidity of a medium-strong acid ψ Z is 10×10 4 ~20×10 4 mmol / m 2 , the acidity of a strong acid ψ Q 0.2×10 4 ~9.5×10 4 mmol / m 2 .
[0009] Furthermore, along the flow direction of the liquid phase reactants, based on the total amount of the three ligands of aluminum in the alumina carrier, the content of the penta-coordinated aluminum ion It decreases gradually, with the decreasing range being 5 to 15 percentage points.
[0010] Furthermore, along the flow direction of the liquid phase reactants, based on the total amount of the three ligands of aluminum in the alumina carrier, the content of the tetracoordinated aluminum ion There are no specific requirements and it can be increased, decreased or unchanged.
[0011] Furthermore, in the alumina carrier of each stage of hydrogenation catalyst, the content of penta-coordinated aluminum ions is based on the total content of the three ligand aluminums. The content of tetracoordinate aluminum ions is 40% to 60%. The content of tri-coordinated aluminum ions is 20% to 50%. It is 10% to 35%.
[0012] Furthermore, the content of pentacoordinated aluminum ions in the alumina support of any stage hydrogenation catalyst is ≥Tetracoordinated aluminum ion content ≥Tricoordinated aluminum ion content
[0013] Furthermore, in the alumina carrier of any one-stage hydrogenation catalyst, the difference between the content of penta-coordinated aluminum ions and the content of tri-coordinated aluminum ions is 15% to 50%.
[0014] Furthermore, the contents of various types of coordinated aluminum ions are calculated as shown in formulas Ⅰ, Ⅱ, and Ⅲ:
[0015]
[0016]
[0017]
[0018] where θ represents the molar number of coordinated aluminum ions, is the coordinated aluminum ion content.
[0019] Furthermore, the n is preferably 3, that is, the graded system contains three catalysts. Based on the total volume of the hydrogenation catalyst in the reactor, the three-stage filling ratios along the flow direction of the liquid reactants are 10% to 90%: 5% to 40%: 5% to 80%, and the sum of the filling ratios of each level is 100%.
[0020] Furthermore, the n is preferably 4, that is, the graded system comprises four hydrogenation catalysts. Based on the total volume of the hydrogenation catalyst in the reactor, along the flow direction of the liquid phase reactants, the four-stage filling ratio is: 10% to 70%: 10% to 40%: 10% to 40%: 10% to 70%, and the sum of the filling ratios of each stage is 100%; the preferred filling ratios are: 10% to 40%: 10% to 40%: 10% to 40%: 10% to 40%, and the sum of the filling ratios of each stage is 100%.
[0021] Furthermore, the hydrogenation catalyst includes an active metal component.
[0022] Furthermore, the alumina carrier is prepared by molding / modifying hydrated alumina and / or alumina composition; wherein the hydrated alumina and / or alumina composition contains tri-coordinated aluminum ions, tetra-coordinated aluminum ions and penta-coordinated aluminum ions, and the acid on the surface of the hydrated alumina and / or alumina composition is a weak acid C R , medium strong acid C Z and strong acid C Q .
[0023] Furthermore, the hydrogenation catalyst is preferably an oxidized hydrogenation catalyst before sulfurization; further preferably, it is a heavy oil hydrogenation catalyst commonly used in the art, wherein, along the flow direction of the reactants, the pore volume of each hydrogenation catalyst decreases step by step, the pore size decreases step by step, the activity increases step by step, and the particle size decreases step by step, such as a hydrodesulfurization agent, a hydrodecarbonization agent, a hydrodenitrogenation agent, etc.
[0024] Furthermore, the hydrogenation catalyst uses Group VIII and / or Group VIB metal elements as active metal components, and based on the weight of the hydrogenation catalyst, the active metal is calculated as oxide, the Group VIII metal content is 0.2wt% to 9.0wt%, preferably 0.5wt% to 9.0wt%, and the Group VIB metal content is 3wt% to 50wt%, preferably 4wt% to 45wt%.
[0025] Furthermore, in the hydrogenation catalyst, the content of the alumina carrier is 45wt% to 96wt%, preferably 50wt% to 95.5wt%, based on the weight of the hydrogenation catalyst.
[0026] Furthermore, in the alumina carrier, the control of the content of different coordinated aluminum mainly depends on the carbonization temperature during the preparation of the alumina carrier. Increasing the carbonization temperature increases the content of penta-ligand aluminum, while decreasing the carbonization temperature increases the content of tri-ligand aluminum.
[0027] Furthermore, the content of different coordinated aluminum in the alumina carrier can also be controlled by adjusting the pH value during the preparation process of the alumina carrier.
[0028] Furthermore, the content of the acid of different strengths on the surface of the alumina carrier is mainly controlled by regulating the mass fraction of organic matter in the organic solution used for the carbonization treatment of different alumina carriers and the temperature of the carbonization treatment during the carbonization treatment.
[0029] Furthermore, the carbonization treatment temperature during the preparation of the alumina carrier is 300-1000°C.
[0030] Furthermore, it is preferred that the hydrogenation catalyst grading system includes three-stage hydrogenation catalysts, and the three-stage hydrogenation catalysts all contain alumina carriers, namely: alumina carrier I, alumina carrier II and alumina carrier III, wherein the carbonization treatment temperature of alumina carrier I is preferably 700-1000°C, and the carbonization treatment time is 2-10h; the carbonization treatment temperature of alumina carrier II is preferably 500-800°C, and the carbonization treatment time is 2-10h; the carbonization treatment temperature of alumina carrier III is preferably 300-500°C, and the carbonization treatment time is 2-10h.
[0031] In the method of the present invention, the synthesis method of alumina used in the alumina carrier I refers to the reaction for preparing aluminum hydroxide gel, which can be specifically one or more of precipitation method (including acid method and alkali method), hydrolysis method, etc. The precipitation method can be one or more of aluminum sulfate method, carbonization method, aluminum chloride method, aluminum nitrate method, etc.; the hydrolysis method can be the hydrolysis reaction of aluminum-containing compounds, such as the hydrolysis of low-carbon aluminum alcohol and high-carbon aluminum alcohol. The prepared alumina raw material is kneaded and extruded into a plastic body, and dried to obtain the desired alumina carrier precursor, the drying temperature is 100-200°C, the drying time is 2-10 hours, and the obtained alumina carrier precursor is carbonized in an atmosphere furnace, the carbonizing agent is an organic solution, including one or more organic solutions such as organic alcohol, organic acid, organic amine, etc., the organic alcohol is preferably selected from ethylene glycol, diethylene glycol or glycerol, the organic acid is preferably selected from oxalic acid, acetic acid, oxalic acid, the organic amine is preferably selected from ethylenediamine, hexamethylenediamine, amino acid (such as glutamic acid), wherein the mass fraction of organic matter in the organic solution is 30wt%-50wt%. After carbonization, the C content in the alumina carrier I is 30wt%-60wt% (based on the alumina carrier), the carbonization treatment temperature is 700-1000°C, and the carbonization treatment time is 2-10 hours.
[0032] In the method of the present invention, the synthesis method of alumina used in the alumina carrier II refers to the reaction for preparing aluminum hydroxide gel, which can be specifically one or more of precipitation method (including acid method and alkali method), hydrolysis method, etc. The precipitation method can be one or more of aluminum sulfate method, carbonization method, aluminum chloride method, aluminum nitrate method, etc.; the hydrolysis method can be a hydrolysis reaction of aluminum-containing compounds, such as the hydrolysis of low-carbon aluminum alcohol and high-carbon aluminum alcohol. Then the prepared alumina raw material is extruded into a plastic body, and dried to obtain the desired alumina carrier precursor, the drying temperature is 100-200°C, the drying time is 2-10 hours, the obtained alumina carrier precursor is carbonized in an atmosphere furnace, the carbonizing agent is an organic solution, including one or more of organic alcohols, organic acids, organic amines and other organic substances, the organic alcohol is preferably selected from ethylene glycol, diethylene glycol or glycerol, the organic acid is preferably selected from oxalic acid, acetic acid, oxalic acid, the organic amine is preferably selected from ethylenediamine, hexamethylenediamine, amino acids (such as glutamic acid), wherein the mass fraction of organic matter in the organic solution is 10wt%-25wt%. After carbonization, the C content in the alumina carrier II is 6wt%-25wt% (based on the alumina carrier), the carbonization temperature is 500-800°C, and the carbonization time is 2-10 hours.
[0033] In the method of the present invention, the synthesis method of alumina used in the alumina carrier III refers to the reaction for preparing aluminum hydroxide gel, which can be specifically one or more of precipitation method (including acid method and alkali method), hydrolysis method, etc. The precipitation method can be one or more of aluminum sulfate method, carbonization method, aluminum chloride method, aluminum nitrate method, etc.; the hydrolysis method can be a hydrolysis reaction of aluminum-containing compounds, such as the hydrolysis of low-carbon aluminum alcohol and high-carbon aluminum alcohol. The prepared alumina raw material is kneaded and extruded into a plastic body, and finally dried and calcined to obtain the desired alumina carrier precursor, the drying temperature is 100-200°C, and the drying time is 2-10 hours; the obtained alumina carrier precursor is carbonized in an atmosphere furnace, the carbonizing agent is an organic solution, including one or more organic substances such as organic alcohol, organic acid, organic amine, etc., the organic alcohol is preferably selected from ethylene glycol, diethylene glycol or glycerol, the organic acid is preferably selected from oxalic acid, oxalic acid, acetic acid, the organic amine is preferably selected from ethylenediamine, hexamethylenediamine, amino acid (such as glutamic acid), wherein the mass fraction of organic matter in the organic solution is 1wt%-5wt%. After carbonization, the C content in the alumina carrier III is 1wt%-5wt% (based on the alumina carrier), the carbonization temperature is 300-500°C, and the carbonization time is 2-10 hours.
[0034] The second aspect of the present invention is to provide an application of the aforementioned hydrogenation catalyst grading method in the hydrogenation treatment of inferior raw materials.
[0035] Furthermore, the inferior raw materials include: heavy inferior raw materials such as gasoline, diesel, wax oil, residual oil, coal tar, coal liquefied oil, etc., especially residual oil raw materials.
[0036] In the method of the present invention, the hydrogenation catalyst in the graded system is preferably vulcanized before use, and the vulcanization method can be wet vulcanization or dry vulcanization.
[0037] Furthermore, the catalyst grading method of the present invention can be used under any hydroprocessing reaction conditions suitable in the art.
[0038] Furthermore, the hydroprocessing reaction conditions are: average reaction temperature of 200°C to 450°C, preferably 250°C to 430°C; reaction hydrogen partial pressure of 4.0MPa to 20.0MPa, preferably 8.0MPa to 18.0MPa; liquid hourly volume space velocity of 0.15h- 1 ~3.0h- 1 , preferably 0.2h- 1 ~2.0h- 1 ; The volume ratio of hydrogen to oil is 300 to 1500, preferably 500 to 1200.
[0039] Compared with the prior art, the method of the present invention has the following advantages:
[0040] In the method of the present invention, along the flow direction of reactants, the modified alumina carrier in the hydrogenation catalyst firstly used has a higher content of penta-coordinated aluminum ions, a moderate content of tetra-coordinated aluminum ions, a lower content of tri-coordinated aluminum ions, a higher content of weak acids, a lower content of strong acids, and a moderate content of medium-strong acids, which weakens the interaction between metal and alumina defects and the interaction between hydrogen and the surface of alumina, thereby increasing hydrogen overflow on the catalyst surface. The overflow hydrogen can enhance the catalytic performance of the catalyst, inhibit the deactivation of the catalyst, and enable the removal of more metals such as Ni, Fe, V, etc., and reduce the carbon on the surface; the modified alumina carrier in the hydrogenation catalyst finally used has a reduced content of penta-coordinated aluminum ions, a moderate content of tetra-coordinated aluminum ions, an increased content of tri-coordinated aluminum ions, a reduced content of weak acids, an increased content of strong acids, enhanced interactions between metal and alumina defects, increased active sites, and reduced steric hindrance of reactants, thereby facilitating the removal of impurities such as O, S, N, etc. that are difficult to remove in small molecules. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The NMR analysis results of the alumina carrier I of the catalyst used in Example 1;
[0042] Figure 2 The NMR analysis result of the alumina carrier II of the catalyst used in Example 1;
[0043] Figure 3This is the nuclear magnetic resonance analysis result of the alumina carrier III of the catalyst used in Example 1. DETAILED DESCRIPTION
[0044] The preparation method of the catalyst of the present invention is described in more detail below through specific examples. The examples are only illustrative of the specific implementation of the method of the present invention and do not constitute a limitation on the scope of protection of the present invention.
[0045] Unless otherwise specified in the present invention, the content of coordinated aluminum ions is molar content.
[0046] In the present invention, a Bruker AVANCE III 500 nuclear magnetic resonance spectrometer is used to determine the type and quantity of aluminum ions. Experimental conditions: BBO normal phase observation broadband probe, H decoupling, deuterium lock channel; standard broadband range: BB = 31P-15N; sensitivity: 367S / N1H NMR, 0.1EB 263S / N 13C NMR, ASTM; resolution: 0.38HZ1 H, 0.1CHCL3, 0.13 13CNMR, ASTM.
[0047] In the method of the present invention, the C content in the alumina carrier after carbonization is determined by a KY-300CS infrared carbon-sulfur analyzer. The minimum detection line of carbon content is 0.01%, power supply: 220V, 50HZ, ambient temperature: 5-40°C, ambient humidity ≤80%RH.
[0048] In the method of the present invention, the specific surface area and pore structure of the hydrogenation catalyst are determined by AUTOSORB-3B low temperature liquid nitrogen adsorption method. The instrument parameters are: specific surface area: >0.05m 2 / g, the gas used is N2, and the pore size range is: 0.35nm-400nm.
[0049] Among the present invention, the instrument adopted is AUTOCHEM 2920-MS, and the acidity of the sample surface is measured by NH3-TPD. Ammonia is adopted as the adsorption and desorption medium, and helium (purity is 99.99v%) is used as the carrier gas, and the acid amount in different desorption temperature zones, i.e. weak acid amount, medium-strong acid amount, strong acid amount and total acid amount, is obtained by temperature program desorption and chromatographic analysis. The specific operation process is as follows: 0.1g of alumina carrier sample of 20-40 meshes is taken, and in the presence of helium (helium flow rate is 30mL / min), the temperature is raised to 500°C, constant temperature is 1 hour, and then it is reduced to 150°C, constant temperature is 5 minutes. Afterwards, ammonia is passed until the alumina carrier is saturated with adsorption, and it is switched to continuous purge of helium (helium flow rate is 30mL / min), the heating rate is 10°C / minute, the temperature is raised to 250°C, constant temperature is 1 hour, and then the temperature is raised to 400°C, constant temperature is 1 hour, and then the temperature is raised to 500°C, constant temperature is 1 hour. During the ammonia desorption process, the ammonia desorption spectrum is recorded by the spectrometer. The obtained ammonia desorption spectrum is divided into three temperature zones according to the desorption temperature, namely 25℃~200℃, 200℃~400℃, and >400℃, which correspond to the acidity of weak acid, medium-strong acid and strong acid respectively. The sum of the acidity of weak acid, medium-strong acid and strong acid is the total acidity. The unit of acidity is: mmol / m 2 , that is, the number of moles of ammonia adsorbed per square meter of carrier surface.
[0050] Example 1
[0051] This embodiment provides a catalyst grading solution for long-term operation of inferior raw materials, that is, loading catalysts in the reactor, and loading hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom along the flow direction of liquid reactants, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 50%:25%:25%.
[0052] The modified alumina used in the hydrogenation catalyst I is prepared by hydrolyzing aluminum sulfate, kneading and extruding into a plastic body, and then drying at 120°C for 3 hours, and then carbonizing in an atmosphere furnace at 950°C for 3.5 hours with 45wt% ethylene glycol vapor to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 58%, and the content of tetracoordinate aluminum ions is Ф IV The value is 30%, and the content of tri-coordinated aluminum ions is Ф III The value is 12%; the surface of alumina carrier I is weakly acidic C R The amount of acid is 27×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 20×10 4 mmol / m 2 , strong acid C Q The amount of acid is 0.3×10 4mmol / m 2 The above-mentioned carrier was saturated with Mo-Ni active metal solution, then dried at 120°C for 3h and calcined at 500°C for 3h to obtain hydrogenation catalyst I. The mass content of MoO3 in hydrogenation catalyst I is 6.2%, the mass content of NiO is 0.9%, the content of alumina carrier I is 92.9%, and the content of C in alumina carrier I is 55%; the properties of hydrogenation catalyst I are as follows: specific surface area is 105m 2 / g, and the pore diameter is 18.8nm.
[0053] The modified alumina used in the hydrogenation catalyst II is prepared by the aluminum sulfate method. After urea is added during the kneading process and extruded into a plastic body, it is dried at 120°C for 2 hours, and then carbonized in an atmosphere furnace at 750°C for 2.5 hours with 12wt% ethylene glycol vapor to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 52%, and the content of tetracoordinate aluminum ions is Ф IV The value is 33%, and the tri-coordinated aluminum ion content Ф III The value is 15%; the surface of alumina carrier II is weakly acidic C R The amount of acid is 19×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 15×10 4 mmol / m 2 , strong acid C Q The amount of acid is 3.8×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 150°C for 2h and calcined at 480°C for 3h to obtain hydrogenation catalyst II. The mass content of MoO3 in hydrogenation catalyst II is 12.5%, the mass content of NiO is 2.7%, the content of alumina carrier II is 84.8%, and the content of C in alumina carrier II is 25%; the properties of hydrogenation catalyst II are as follows: specific surface area is 165m 2 / g, and the pore diameter is 13.8nm.
[0054] The modified alumina used in the hydrogenation catalyst III is prepared from aluminum sulfate, which is kneaded and extruded into a plastic body and then dried at 150°C for 2 hours. Then, it is carbonized in an atmosphere furnace at 450°C for 3 hours with ethylene glycol vapor at a concentration of 2wt% to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 45%, and the content of tetracoordinate aluminum ions is Ф IV The value is 35%, and the tri-coordinated aluminum ion content Ф III The value is 20%; the surface of alumina carrier III is weakly acidic C R The amount of acid is 10×104 mmol / m 2 , medium strong acid C Z The amount of acid is 10×10 4 mmol / m 2 , strong acid C Q The amount of acid is 7.6×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 180°C for 3h and calcined at 400°C for 5h to obtain hydrogenation catalyst III. The mass content of MoO3 in hydrogenation catalyst III is 23.5%, the mass content of NiO is 3.8%, the content of alumina carrier III is 72.7%, and the C content in alumina carrier III is 2.5%; the properties of hydrogenation catalyst III are as follows: specific surface area is 175m 2 / g, and the pore diameter is 8.8nm.
[0055] Example 2
[0056] This embodiment provides a catalyst grading solution for long-term operation of inferior raw materials, that is, loading catalysts in the reactor, and loading hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom along the flow direction of liquid reactants in the bed, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 50%:30%:20%.
[0057] The modified alumina used in the hydrogenation catalyst I is prepared by hydrolyzing aluminum isopropoxide, kneaded and extruded into a plastic body, and then dried at 150°C for 3 hours, and then carbonized in an atmosphere furnace at 900°C for 3 hours with 50wt% diethylene glycol vapor to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 50%, the content of tetracoordinated aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III Value is 10%; weak acid C R The amount of acid is 29×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 18×10 4 mmol / m 2 , strong acid C Q The amount of acid is 0.5×10 4 mmol / m 2The above-mentioned carrier was saturated with Mo-Ni active metal solution, then dried at 120°C for 5h and calcined at 470°C for 2h to obtain hydrogenation catalyst I. The mass content of MoO3 in hydrogenation catalyst I is 5.5%, the mass content of NiO is 0.8%, the content of alumina carrier I is 93.7%, and the C content in alumina carrier I is 59%; the properties of hydrogenation catalyst I are as follows: specific surface area is 120m 2 / g, and the pore diameter is 17.9nm.
[0058] The modified alumina used in the hydrogenation catalyst II is prepared by hydrolyzing aluminum isopropoxide, and after adding ethylenediamine during the kneading process to extrude into a plastic body, it is dried at 120°C for 2 hours, and then carbonized in an atmosphere furnace at 650°C for 3 hours with 20wt% glycerol vapor to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 45%, and the content of tetracoordinate aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 15%; weak acid C R The amount of acid is 20×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 15×10 4 mmol / m 2 , strong acid C Q The amount of acid is 2.9×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 180°C for 3h and calcined at 470°C for 4h to obtain hydrogenation catalyst II. The mass content of MoO3 in hydrogenation catalyst II is 13.5%, the mass content of NiO is 2.6%, the content of alumina carrier II is 83.9%, and the C content in alumina carrier II is 20%; the properties of hydrogenation catalyst II are as follows: specific surface area is 166m 2 / g, and the pore diameter is 12.8nm.
[0059] The modified alumina used in the hydrogenation catalyst III is prepared by hydrolyzing aluminum isopropoxide, kneaded and extruded into a plastic body, dried at 150°C for 2 hours, and then carbonized at 500°C for 3 hours in an atmosphere furnace with 5wt% ethylenediamine vapor to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 40%, and the content of tetracoordinate aluminum ions is Ф IV The value is 35%, and the tri-coordinated aluminum ion content Ф III Value is 25%; weak acid C R The amount of acid is 15×10 4 mmol / m 2, medium strong acid C Z The amount of acid is 12×10 4 mmol / m 2 , strong acid C Q The amount of acid is 7.6×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 150°C for 2h and calcined at 400°C for 3h to obtain hydrogenation catalyst III. The mass content of MoO3 in hydrogenation catalyst III is 23.5%, the mass content of NiO is 3.7%, the content of alumina carrier III is 72.8%, and the C content in alumina carrier III is 1.5%; the properties of hydrogenation catalyst III are as follows: specific surface area is 190m 2 / g, and the pore diameter is 8.9nm.
[0060] Example 3
[0061] This embodiment provides a catalyst grading solution for long-term operation of inferior raw materials, that is, loading catalysts in the reactor, and loading hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom along the flow direction of liquid reactants in the bed, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 15%:25%:60%.
[0062] The modified alumina used in the hydrogenation catalyst I is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 200°C for 3 hours, and then carbonized in an atmosphere furnace at 850°C for 4.0 hours with 35wt% ethylenediamine vapor to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 60%, and the content of tetracoordinated aluminum ions is Ф IV The value is 30%, and the tri-coordinated aluminum ion content Ф III Value is 10%; weak acid C R The amount of acid is 25×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 17×10 4 mmol / m 2 , strong acid C Q The amount of acid is 1.0×10 4 mmol / m 2 The above-mentioned carrier was saturated with Mo-Ni active metal solution, then dried at 140°C for 2h and calcined at 520°C for 4h to obtain hydrogenation catalyst I. The mass content of MoO3 in hydrogenation catalyst I is 4.2%, the mass content of NiO is 0.6%, the content of alumina carrier I is 95.2%, and the content of C in alumina carrier I is 50%; the properties of hydrogenation catalyst I are as follows: the specific surface area is 121m 2 / g, and the pore diameter is 21.7nm.
[0063] The modified alumina used in the hydrogenation catalyst II is prepared by carbonization. After diethylene glycol is added during the kneading process to extrude into a plastic body, it is dried at 120°C for 2 hours, and then carbonized in an atmosphere furnace at 750°C for 3 hours with 25wt% oxalic acid vapor to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 54%, and the content of tetracoordinate aluminum ions is Ф IV The value is 30%, and the tri-coordinated aluminum ion content Ф III The value is 16%; weak acid C R The amount of acid is 22×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 14×10 4 mmol / m 2 , strong acid C Q The amount of acid is 3.9×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 160°C for 3h and calcined at 490°C for 4h to obtain hydrogenation catalyst II. The mass content of MoO3 in hydrogenation catalyst II is 13.3%, the mass content of NiO is 1.8%, the content of alumina carrier II is 84.9%, and the C content in alumina carrier II is 19%; the properties of hydrogenation catalyst II are as follows: specific surface area is 150m 2 / g, and the pore diameter is 15.6nm.
[0064] The modified alumina used in the hydrogenation catalyst III is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours, and then carbonized in an atmosphere furnace at 450°C for 2.5 hours with 6wt% ethylene glycol vapor to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 42%, and the content of tetracoordinate aluminum ions is Ф IV The value is 38%, and the tri-coordinated aluminum ion content Ф III Value is 20%; weak acid C R The amount of acid is 17×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 12×10 4 mmol / m 2 , strong acid C Q The amount of acid is 8.9×10 4 mmol / m 2The above carrier was saturated with Mo-Ni active metal solution, then dried at 150°C for 3h and calcined at 450°C for 3h to obtain hydrogenation catalyst III. The mass content of MoO3 in hydrogenation catalyst III is 23.3%, the mass content of NiO is 3.8%, the content of alumina carrier III is 72.9%, and the C content in alumina carrier III is 1.2%; the properties of hydrogenation catalyst III are as follows: specific surface area is 221m 2 / g, and the pore diameter is 10.2nm.
[0065] Example 4
[0066] This embodiment provides a catalyst grading solution for long-term operation of inferior raw materials, that is, loading catalysts in the reactor, and loading hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III in the bed from top to bottom, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 15%:25%:60%.
[0067] The modified alumina used in the hydrogenation catalyst I is prepared by carbonization, and after being kneaded and extruded into a plastic body, it is dried at 220°C for 4 hours and then carbonized in an atmosphere furnace at 850°C for 5 hours with 40wt% ethylene glycol vapor to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 59%, and the content of tetracoordinate aluminum ions is Ф IV The value is 30%, and the tri-coordinated aluminum ion content Ф III The value is 11%; weak acid C R The amount of acid is 30×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 19×10 4 mmol / m 2 , strong acid C Q The amount of acid is 0.2×10 4 mmol / m 2 The above-mentioned carrier was saturated with Mo-Ni active metal solution, then dried at 150°C for 3h and calcined at 400°C for 2h to obtain hydrogenation catalyst I. The mass content of MoO3 in hydrogenation catalyst I is 4.3%, the mass content of NiO is 0.8%, the content of alumina carrier I is 94.9%, and the C content in alumina carrier I is 58%; the properties of hydrogenation catalyst I are as follows: specific surface area is 115m 2 / g, and the pore diameter is 22.7nm.
[0068] The modified alumina used in the hydrogenation catalyst II is prepared by carbonization. After adding citric acid during the kneading process to extrude into a plastic body, it is dried at 180°C for 4 hours, and then carbonized in an atmosphere furnace at 700°C for 3 hours with 12wt% propylene glycol vapor to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 53%, and the content of tetracoordinate aluminum ions is Ф IV The value is 27%, and the content of tri-coordinated aluminum ions is Ф III Value is 20%; weak acid C R The amount of acid is 22×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 14×10 4 mmol / m 2 , strong acid C Q The amount of acid is 3.7×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 120°C for 3h and calcined at 450°C for 3h to obtain hydrogenation catalyst II. The mass content of MoO3 in hydrogenation catalyst II is 11.3%, the mass content of NiO is 2.0%, the content of alumina carrier II is 86.7%, and the C content in alumina carrier II is 20%; the properties of hydrogenation catalyst II are as follows: specific surface area is 166m 2 / g, and the pore diameter is 16.2nm.
[0069] The modified alumina used in the hydrogenation catalyst III is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 120°C for 3 hours, and then treated with 2wt% ethylene glycol vapor at 480°C for 2 hours in an atmosphere furnace to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 42%, and the content of tetracoordinate aluminum ions is Ф IV The value is 33%, and the tri-coordinated aluminum ion content Ф III Value is 25%; weak acid C R The amount of acid is 18×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 14×10 4 mmol / m 2 , strong acid C Q The amount of acid is 9.4×10 4 mmol / m 2The above carrier was saturated with Mo-Ni active metal solution, then dried at 180°C for 3h and calcined at 480°C for 3h to obtain hydrogenation catalyst III. The mass content of MoO3 in hydrogenation catalyst III is 22.3%, the mass content of NiO is 3.5%, the content of alumina carrier III is 74.2%, and the C content in alumina carrier III is 2.0%; the properties of hydrogenation catalyst III are as follows: specific surface area is 215m 2 / g, and the pore diameter is 10.2nm.
[0070] Example 5
[0071] This embodiment provides a catalyst grading solution for long-term operation with inferior raw materials, that is, loading catalysts in the reactor, and loading hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III in the bed from top to bottom, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 30%:35%:35%.
[0072] The modified alumina used in the hydrogenation catalyst I is prepared by carbonization, and after being mixed and kneaded into a plastic body, it is dried at 220°C for 4 hours and then carbonized in an atmosphere furnace at 900°C for 4 hours with 35wt% oxalic acid vapor to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 58%, and the content of tetracoordinate aluminum ions is Ф IV The value is 28%, and the tri-coordinated aluminum ion content Ф III The value is 14%; weak acid C R The amount of acid is 28×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 18×10 4 mmol / m 2 , strong acid C Q The amount of acid is 0.5×10 4 mmol / m 2 The above-mentioned carrier was saturated with Mo-Ni active metal solution, then dried at 120°C for 3h and calcined at 500°C for 3h to obtain hydrogenation catalyst I. The mass content of MoO3 in hydrogenation catalyst I is 4.5%, the mass content of NiO is 0.7%, the content of alumina carrier I is 94.8%, and the C content in alumina carrier I is 54%; the properties of hydrogenation catalyst I are as follows: specific surface area is 105m 2 / g, and the pore diameter is 23.6nm.
[0073] The modified alumina used in the hydrogenation catalyst II is prepared by carbonization. After adding polypropylene alcohol during the kneading process to extrude into a plastic body, it is dried at 150°C for 4 hours, and then carbonized in an atmosphere furnace at 690°C for 4 hours with 16wt% glutamic acid vapor to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 52%, and the content of tetracoordinate aluminum ions is Ф IV The value is 27%, and the content of tri-coordinated aluminum ions is Ф III The value is 21%; weak acid C R The amount of acid is 21×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 15×10 4 mmol / m 2 , strong acid C Q The amount of acid is 3.9×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 150°C for 3h and calcined at 400°C for 3h to obtain hydrogenation catalyst II. The mass content of MoO3 in hydrogenation catalyst II was 12.4%, the mass content of NiO was 2.1%, the content of alumina carrier II was 85.5%, and the C content in alumina carrier II was 19%; the properties of hydrogenation catalyst II are as follows: specific surface area is 156m 2 / g, and the pore diameter is 17.2nm.
[0074] The modified alumina used in the hydrogenation catalyst III is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 120°C for 3 hours, and then treated with 3wt% ethylenediamine vapor at 500°C for 2.5 hours in an atmosphere furnace to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 45%, and the content of tetracoordinate aluminum ions is Ф IV The value is 22%, and the tri-coordinated aluminum ion content Ф III The value is 33%; weak acid C R The amount of acid is 20×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 16×10 4 mmol / m 2 , strong acid C Q The amount of acid is 8.9×10 4 mmol / m 2The above carrier was saturated with Mo-Ni active metal solution, then dried at 180°C for 3h and calcined at 450°C for 3h to obtain hydrogenation catalyst III. The mass content of MoO3 in hydrogenation catalyst III is 24.3%, the mass content of NiO is 3.9%, the content of alumina carrier III is 71.8%, and the C content in alumina carrier III is 1.4%; the properties of hydrogenation catalyst III are as follows: specific surface area is 225m 2 / g, and the pore diameter is 12.2nm.
[0075] Comparative Example 1
[0076] This example provides a catalyst grading solution for long-term operation with inferior raw materials, namely, loading catalysts in the reactor, with the bed layer loaded with hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 50%:25%:25%.
[0077] The modified alumina used in the hydrogenation catalyst I is prepared by hydrolyzing aluminum isopropoxide, and after being mixed and kneaded into a plastic body, it is dried at 120°C for 3 hours, and then treated with 70wt% ethylene glycol vapor at 900°C for 3 hours in an atmosphere furnace to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 55%, and the content of tetracoordinated aluminum ions is Ф IV The value is 35%, and the tri-coordinated aluminum ion content Ф III Value is 10%; weak acid C R The amount of acid is 50×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 20×10 4 mmol / m 2 , strong acid C Q The amount of acid is 0.1×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 120°C for 3h, and calcined at 500°C for 3h. The prepared catalyst had a MoO3 mass content of 6.5%, a NiO mass content of 0.7%, alumina carrier I content of 92.8%, and a C content of 69% in alumina carrier I. The properties of the catalyst are as follows: specific surface area of 110m 2 / g, and the pore diameter is 18.8nm.
[0078] The modified alumina used in the hydrogenation catalyst II is prepared by the aluminum sulfate method. After urea is added during the kneading process and extruded into a plastic body, it is dried at 120°C for 2 hours, and then carbonized in an atmosphere furnace at 700°C for 3 hours with 12wt% ethylene glycol vapor to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 45%, and the content of tetracoordinate aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 15%; weak acid C R The amount of acid is 20×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 18×10 4 mmol / m 2 , strong acid C Q The amount of acid is 4.1×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 150°C for 4h, and calcined at 450°C for 3h. The prepared catalyst had a MoO3 mass content of 12.0%, a NiO mass content of 2.5%, an alumina carrier II content of 85.5%, and a C content of 15% in the alumina carrier II. The properties of the catalyst are as follows: specific surface area of 179m 2 / g, and the pore diameter is 12.1nm.
[0079] The modified alumina used in the hydrogenation catalyst III is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours, and then carbonized in an atmosphere furnace at 500°C for 3 hours with 0.1wt% ethylene glycol vapor to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 40%, and the content of tetracoordinate aluminum ions is Ф IV The value is 35%, and the tri-coordinated aluminum ion content Ф III Value is 25%; weak acid C R The amount of acid is 5×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 20×10 4 mmol / m 2 , strong acid C Q The amount of acid is 15.0×10 4 mmol / m 2The above carrier was saturated with Mo-Ni active metal solution, then dried at 160°C for 3h, and calcined at 510°C for 3h. The prepared catalyst had a MoO3 mass content of 21.5%, a NiO mass content of 3.6%, a content of 74.9% in alumina carrier III, and a C content of 2.3% in alumina carrier III. The properties of the catalyst are as follows: the specific surface area is 200m 2 / g, and the pore diameter is 8.9nm.
[0080] Comparative Example 2
[0081] This example provides a catalyst grading solution for long-term operation with inferior raw materials, namely, loading catalysts in the reactor, with the bed layer loaded with hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 15%:25%:60%.
[0082] The modified alumina used in the hydrogenation catalyst I is prepared by hydrolyzing aluminum isopropoxide, and after being kneaded and extruded into a plastic body, it is dried at 200°C for 3 hours, and then carbonized in an atmosphere furnace at 800°C for 3 hours with 5wt% ethylene glycol vapor to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 10%, the content of tetracoordinated aluminum ions Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III Value is 50%; weak acid C R The amount of acid is 19×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 11×10 4 mmol / m 2 , strong acid C Q The amount of acid is 8.9×10 4 mmol / m 2 . . The above carrier was saturated with Mo-Ni active metal solution, then dried at 150°C for 3h and calcined at 400°C for 3h to obtain hydrogenation catalyst I. The mass content of MoO3 in hydrogenation catalyst I was 4.3%, the mass content of NiO was 0.7%, the content of alumina carrier I was 95%, and the C content in alumina carrier I was 53%; the properties of the catalyst are as follows: the specific surface area is 116m 2 / g, and the pore diameter is 23.7nm.
[0083] The modified alumina used in the hydrogenation catalyst II is prepared by the aluminum sulfate method. After adding diethylene glycol during the kneading process, it is extruded into a plastic body and then dried at 120°C for 2 hours. Then, it is carbonized in an atmosphere furnace at 700°C for 3 hours with 20wt% ethylene glycol vapor to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 45%, and the content of tetracoordinate aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 15%; weak acid C R The amount of acid is 25×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 17×10 4 mmol / m 2 , strong acid C Q The amount of acid is 3.5×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 180°C for 3h and calcined at 450°C for 3h to obtain hydrogenation catalyst II. The mass content of MoO3 in hydrogenation catalyst II is 12.3%, the mass content of NiO is 1.9%, the content of alumina carrier II is 85.8%, and the C content in alumina carrier II is 16%; the properties of the catalyst are as follows: the specific surface area is 142m 2 / g, and the pore diameter is 17.2nm.
[0084] The modified alumina used in the hydrogenation catalyst III is prepared by carbonization, and after being kneaded and extruded into a plastic body, it is dried at 150°C for 2 hours, and then carbonized in an atmosphere furnace at 500°C for 3 hours with 45wt% ethylenediamine vapor to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 20%, and the content of tetracoordinate aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III Value is 40%; weak acid C R The amount of acid is 27×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 19×10 4 mmol / m 2 , strong acid C Q The amount of acid is 0.2×10 4 mmol / m 2The above carrier was saturated with Mo-Ni active metal solution, then dried at 160°C for 3h and calcined at 480°C for 3h to obtain hydrogenation catalyst III. The mass content of MoO3 in hydrogenation catalyst III is 20.3%, the mass content of NiO is 3.6%, the content of alumina carrier III is 76.1%, and the C content in alumina carrier III is 2.5%; the properties of the catalyst are as follows: the specific surface area is 221m 2 / g, and the pore diameter is 10.2nm.
[0085] Comparative Example 3
[0086] This example provides a catalyst grading solution for long-term operation with inferior raw materials, namely, loading catalysts in the reactor, with the bed layer loaded with hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 15%:25%:60%.
[0087] The modified alumina used in the hydrogenation catalyst I is prepared by the aluminum sulfate method. After diethylene glycol is added during the kneading process to extrude into a plastic body, it is dried at 120°C for 2 hours, and then carbonized in an atmosphere furnace at 700°C for 3 hours with 15wt% ethylene glycol vapor to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 50%, the content of tetracoordinated aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III Value is 10%; weak acid C R The amount of acid is 25×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 17×10 4 mmol / m 2 , strong acid C Q The amount of acid is 0.5×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 150°C for 3h and calcined at 510°C for 4h to obtain hydrogenation catalyst I. The mass content of MoO3 in hydrogenation catalyst I was 4.3%, the mass content of NiO was 0.7%, the content of alumina carrier I was 95%, and the C content in alumina carrier I was 58%; the properties of the catalyst are as follows: the specific surface area is 210m 2 / g, and the pore diameter is 17.6nm.
[0088] The modified alumina used in the hydrogenation catalyst II is prepared by the aluminum sulfate method. After adding diethylene glycol during the kneading process, it is extruded into a plastic body and then dried at 120°C for 2 hours. Then, it is carbonized in an atmosphere furnace at 700°C for 3 hours with 15wt% ethylene glycol vapor to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 50%, the content of tetracoordinated aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III Value is 10%; weak acid C R The amount of acid is 25×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 17×10 4 mmol / m 2 , strong acid C Q The amount of acid is 0.5×10 4 mmol / m 2 The above carrier was saturated with Mo-Ni active metal solution, then dried at 160°C for 3h and calcined at 480°C for 5h to obtain hydrogenation catalyst II. The mass content of MoO3 in hydrogenation catalyst II was 12.3%, the mass content of NiO was 1.9%, the content of alumina carrier II was 85.8%, and the content of C in alumina carrier II was 54%. The properties of the catalyst are as follows: the specific surface area is 176m 2 / g, and the pore diameter is 17.2nm.
[0089] The modified alumina used in the hydrogenation catalyst III is prepared by the aluminum sulfate method. After diethylene glycol is added during the kneading process to extrude into a plastic body, it is dried at 120°C for 2 hours, and then carbonized in an atmosphere furnace at 700°C for 3 hours with 15wt% ethylene glycol vapor to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared alumina carrier III is Φ V The value is 50%, the content of tetracoordinated aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 10%; Weak acid C R The amount of acid is 25×10 4 mmol / m 2 , medium strong acid C Z The amount of acid is 17×10 4 mmol / m 2 , strong acid C Q The amount of acid is 0.5×10 4 mmol / m 2The above carrier was saturated with Mo-Ni active metal solution, then dried at 170°C for 2h and calcined at 450°C for 5h to obtain hydrogenation catalyst III. The mass content of MoO3 in hydrogenation catalyst III is 20.3%, the mass content of NiO is 3.6%, the content of alumina carrier III is 76.1%, and the C content in alumina carrier III is 55%; the properties of the catalyst are as follows: the specific surface area is 141m 2 / g, and the pore diameter is 17.2nm.
[0090] Example 6
[0091] This example is a comparative test of the activity and stability of the catalyst combination system of Examples 1, 2, 3, 4, 5 and Comparative Examples 1, 2, 3 on a 100mL fixed bed small hydrogenation device, and the feeding method adopts upper feeding. The properties of the evaluated raw oil are shown in Table 1; the evaluation conditions are shown in Table 2; the catalyst combination scheme is shown in Table 3; and the evaluation results of the catalyst combination scheme are shown in Table 4.
[0092] Table 1 Raw oil properties
[0093] Crude oil Residue <![CDATA[Density (20 °C), g·cm -3 > 0.9985 Carbon residue, wt% 14.56 S, wt% 6.77 <![CDATA[Ni+V,μg·g -1 ]]> 159.7
[0094] Table 2 Evaluation process conditions
[0095] Reaction temperature, °C 420 Reaction hydrogen partial pressure, MPa 15.5 <![CDATA[Liquid hourly space velocity, h -1 > 0.25 Hydrogen to oil volume ratio 1000:1
[0096] Table 3 Evaluation results of various catalyst combinations
[0097]
[0098] The above describes the specific implementation of the present invention in detail, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the various technical features being combined in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A hydrogenation catalyst grading method, characterized in that: The method comprises a graded system consisting of n-level catalysts, wherein n≥3, and any level of catalyst comprises an alumina carrier, and the surface of the alumina carrier contains three acids of different strengths: weak acid C R , medium strong acid C Z and strong acid C Q The alumina carrier contains three types of aluminum ions: three-coordinate aluminum ions Al 3+ Ⅲ , four-coordinated aluminum ion Al 3+ Ⅳ and pentacoordinated aluminum ion Al 3+ Ⅴ The n-level catalyst grading satisfies the following conditions: along the flow direction of the liquid phase reactant, based on the total amount of the three acids in the alumina carrier, the acidity of the strong acid ψ Q Increase step by step, the increment is 1×10 4 ~9×10 4 mmol / m 2 , the acidity of the weak acid ψ R Decrease gradually, with a decreasing amplitude of 1×10 4 ~20×10 4 mmol / m 2 ; Based on the total amount of three ligands of aluminum in the alumina carrier, the content of tri-coordinated aluminum ions The content of pentacoordinated aluminum ions increases gradually by 1 to 10 percentage points. It decreases gradually, with the decreasing range being 5 to 15 percentage points.
2. The grading method according to claim 1, characterized in that: Along the flow direction of the liquid phase reactants, based on the total amount of the three acids in the alumina carrier, the acidity of the weak acid ψ R Decrease gradually, with a decreasing amplitude of 1×10 4 ~10×10 4 mmol / m 2 , the acidity of a strong acid ψ Q Increase step by step, the increment is 1×10 4 ~7×10 4 mmol / m 2 .
3. The grading method according to claim 1, characterized in that: The catalyst grading method comprises a grading system consisting of n-grade catalysts, wherein n is 3 or 4.
4. The grading method according to claim 1, characterized in that: The amount of weak acid in the alumina support of any stage catalyst is R is 10×10 4 ~30×10 4 mmol / m 2 , the acidity of a medium-strong acid ψ Z is 10×10 4 ~20×10 4 mmol / m 2 , the acidity of a strong acid ψ Q 0.2×10 4 ~9.5×10 4 mmol / m 2 .
5. The grading method according to claim 1, characterized in that: In the alumina carrier of any first-stage catalyst, the content of penta-coordinated aluminum ions is based on the total content of three ligand aluminum. The content of tetracoordinate aluminum ions is 40% to 60%. 20% to 50%, tri-coordinated aluminum ion content It is 10% to 35%.
6. The grading method according to claim 1, characterized in that: In the alumina carrier of the same grade catalyst, 7. The grading method according to claim 1, characterized in that: In the alumina carrier of the same grade of catalyst, the difference between the content of penta-coordinated aluminum ions and the content of tri-coordinated aluminum ions is 15% to 50%.
8. The grading method according to claim 1, characterized in that: The graded system includes three catalysts. Based on the total volume of the catalyst in the reactor, along the flow direction of the liquid phase reactants, the three-level filling ratios are 10% to 90%: 5% to 40%: 5% to 80%, and the sum of the filling ratios of each level is 100%.
9. The grading method according to claim 1, characterized in that: The graded system includes four catalysts. Based on the total volume of the catalyst in the reactor, the four-stage filling ratios along the flow direction of the liquid reactants are: 10% to 70%: 10% to 40%: 10% to 40%: 10% to 70%, and the sum of the filling ratios of each stage is 100%.
10. The grading method according to claim 1, characterized in that: The graded system includes four catalysts. Based on the total volume of the catalyst in the reactor, the four-stage filling ratios along the flow direction of the liquid reactants are: 10% to 40%: 10% to 40%: 10% to 40%: 10% to 40%: 10% to 40%, and the sum of the filling ratios of each stage is 100%.
11. The grading method according to claim 1, characterized in that: In each level of hydrogenation catalyst, the content of the alumina carrier is 45wt% to 96wt% based on the weight of the hydrogenation catalyst.
12. The grading method according to claim 1, characterized in that: In each level of hydrogenation catalyst, the content of the alumina carrier is 50wt% to 95.5wt% based on the weight of the hydrogenation catalyst.
13. Use of the catalyst grading method according to any one of claims 1 to 12 in the hydroprocessing of inferior raw materials.
14. The use according to claim 13, characterized in that The reaction conditions of the hydrotreatment are: average reaction temperature of 200°C to 450°C; reaction hydrogen partial pressure of 4.0MPa to 20.0MPa; liquid hourly volume space velocity of 0.15h -1 ~3.0h -1 ; The volume ratio of hydrogen to oil is 300~1500.
15. The use according to claim 13, characterized in that: The reaction conditions of the hydrotreatment are: average reaction temperature of 250°C to 430°C; reaction hydrogen partial pressure of 8.0MPa to 18.0MPa; liquid hourly volume space velocity of 0.2h -1 ~2.0h -1 ; The volume ratio of hydrogen to oil is 500~1200.