Hydrogenation catalyst grading method and its application

Through multi-stage sulfide hydrogenation catalyst gradation, the catalyst microstructure is optimized to match the molecular structure of the reactants, which solves the problem of impurities in inferior raw materials that make it difficult to operate for a long period of time, improves the activity and utilization of the hydrogenation catalyst, and prolongs the operation of the device. time.

CN116440918BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210012187.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-06
Publication Date
2024-10-15
Estimated Expiration
2042-01-06

AI Technical Summary

Technical Problem

The existing heavy oil hydrogenation catalyst grading method cannot effectively solve the problem of impurities in inferior raw materials that are difficult to operate for a long period of time, resulting in limited hydrogenation reaction depth and low catalyst activity utilization.

Method used

A multi-stage sulfide hydrogenation catalyst gradation system is adopted, in which each stage of the catalyst contains an alumina carrier and a metal active component. By adjusting the type of coordinated aluminum ions, the length and number of active phase lamellae, the microstructure of the catalyst is optimized to match the reaction The molecular structure of the material is adjusted to achieve reasonable distribution of impurities and synchronous deactivation of the catalyst.

Benefits of technology

The activity and utilization rate of the hydrogenation catalyst are improved, the long-term operation time of the device is extended, and the catalytic performance and anti-deactivation ability of the catalyst are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116440918B_ABST
    Figure CN116440918B_ABST
Patent Text Reader

Abstract

The present invention discloses a hydrogenation catalyst grading method and its application. The grading method comprises a multi-stage sulfided hydrogenation catalyst, each stage of the catalyst comprises an alumina carrier and a metal active component, and the alumina carrier contains three types of aluminum ions: tri-coordinated aluminum ions Al 3+ Ⅲ , four-coordinated aluminum ion Al 3+ Ⅳ and pentacoordinated aluminum ion Al 3+ Ⅴ Along the flow direction of the liquid phase reactant, based on the total amount of three ligand aluminum in the alumina carrier, the content of penta-coordinated aluminum ions #imgabs0# decreases step by step, with a step-by-step decrease range of 5 to 15 percentage points, the average length of the metal active phase lamella increases step by step, and the average number of lamellae decreases step by step. The grading method of the present invention is applied to the hydrogenation treatment of inferior raw materials, which can significantly reduce the steric hindrance effect and improve the utilization rate of the active metal phase.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hydrogenation catalyst grading method and application thereof, in particular to a hydrogenation catalyst grading method for heavy oil hydrogenation in long-term operation of inferior raw materials and application thereof. Background Art

[0002] During the heavy oil hydrogenation process, as the raw materials become heavier and inferior, the content of metal impurities and inorganic salts such as Fe, Si, Na, Ca in the raw materials continues to increase. These metals mainly exist in the form of colloids and asphaltene. Secondly, the heavy inferior raw materials have low saturated hydrocarbon content, high aromatic hydrocarbon content, and high colloid content, especially high heavy aromatic hydrocarbon content. These heavy raw materials have complex molecular structures, large steric hindrance, and impurities are easier to remove; with the hydrogenation and hydrogenolysis reactions, the reactant molecules gradually open the ring and break the chain, the molecular structure is gradually simplified, the steric hindrance is small, and impurities are more difficult to remove. At present, the grading method of heavy oil hydrogenation catalyst is often studied from the surface level, that is, the catalyst particle size, pore size and activity transition, and it is not considered from the actual reactant molecular structure level and catalyst microstructure. As the reaction proceeds, the reactant molecular structure and catalyst microstructure cannot match well, which limits the depth of the hydrogenation reaction.

[0003] CN103773437A discloses a grading method for a hydrodesulfurization catalyst, the method comprising: a hydrogenation reactor includes at least two catalyst beds, in accordance with the order of contact with the reaction material, the upstream bed is a low-pile ratio catalyst bed, the downstream catalyst bed has a higher pile ratio than the adjacent upstream catalyst bed; each catalyst bed is graded and loaded with two or more catalysts of different diameters. These physical mixtures have a smaller void ratio and a larger loading pile ratio than their single diameter catalysts, which improves the hydrodesulfurization performance of the entire reaction system, but it is difficult to achieve long-term stable operation for processing inferior raw materials with high solid impurity content. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a grading method for a hydrogenation catalyst to solve the problem of long-term operation of inferior raw materials, to effectively optimize the activity grading of the overall hydrogenation catalyst, to achieve a reasonable distribution of impurities in the entire system, and to achieve the purpose of synchronous deactivation of the entire catalyst system as much as possible, so as to improve the utilization rate of the hydrogenation catalyst and achieve long-term operation of the device.

[0005] To achieve the above object, the present invention provides a hydrogenation catalyst grading method, comprising a grading system consisting of n-level sulfided hydrogenation catalysts, wherein n ≥ 3, preferably n is 3 or 4, each level of sulfided hydrogenation catalyst comprises an alumina carrier and a metal active component, and the alumina carrier contains three types of aluminum ions: tri-coordinated aluminum ions Al 3+Ⅲ , four-coordinated aluminum ion Al 3+ IV and pentacoordinated aluminum ion Al 3+ Ⅴ The content of pentacoordinated aluminum ions in each hydrogenation catalyst along the flow direction of the liquid reactants is based on the total amount of three ligands of aluminum in the alumina carrier. The decrease is 5 to 15 percentage points step by step. The average length of the metal active phase lamellae increases step by step and the average number of lamellae decreases step by step along the flow direction of the liquid phase reactants of each hydrogenation catalyst. The metal active phase is an active metal sulfide.

[0006] Furthermore, the sulfided hydrogenation catalyst is obtained by sulfiding an oxidized hydrogenation catalyst.

[0007] Furthermore, along the flow direction of the liquid phase reactants, the content of the tri-coordinated aluminum ion is based on the total amount of the three ligands of aluminum in the alumina carrier. The increase is gradual, with the increment ranging from 1 to 10 percentage points.

[0008] Furthermore, along the flow direction of the liquid phase reactants, based on the total amount of the three ligands of aluminum in the alumina carrier, the content of the tetracoordinated aluminum ion There are no specific requirements and it can be increased, decreased or unchanged.

[0009] Furthermore, in the alumina carrier of each stage of hydrogenation catalyst, the content of penta-coordinated aluminum ions is based on the total content of the three ligand aluminums. The content of tetracoordinate aluminum ions is 40% to 60%. The content of tri-coordinated aluminum ions is 30% to 50%. It is 10% to 30%.

[0010] Furthermore, the contents of various types of coordinated aluminum ions are calculated as shown in formulas Ⅰ, Ⅱ, and Ⅲ:

[0011]

[0012]

[0013]

[0014] where θ represents the molar number of coordinated aluminum ions, is the coordinated aluminum ion content.

[0015] Furthermore, in the alumina support of the same stage hydrogenation catalyst, the content of pentacoordinated aluminum ions is ≥Tetracoordinated aluminum ion content ≥Tricoordinated aluminum ion content

[0016] Furthermore, in the alumina carrier of the same level of hydrogenation catalyst, the difference between the content of penta-coordinated aluminum ions and the content of tri-coordinated aluminum ions is 15% to 50%.

[0017] Furthermore, in each stage of the sulfided hydrogenation catalyst, the average length of the metal active phase crystal is 1 to 9 nm, and the gradual increase range is 1 to 5 nm, preferably 2 to 4 nm.

[0018] Furthermore, in each level of sulfided hydrogenation catalyst, the average number of metal active phase crystals is 1 to 9, and the amplitude decreases from 1 to 5, preferably from 2 to 4.

[0019] Furthermore, the n is preferably 3, that is, the graded system contains three sulfide hydrogenation catalysts. Based on the total volume of the catalyst in the reactor, along the flow direction of the liquid reactants, the three-stage filling ratio is 10% to 90%: 5% to 40%: 5% to 80%, and the sum of the filling ratios of each level is 100%.

[0020] Furthermore, the n is preferably 4, that is, the graded system comprises four sulfide hydrogenation catalysts. Based on the total volume of the catalyst in the reactor, along the flow direction of the liquid phase reactants, the four-stage filling ratio is: 10% to 70%: 10% to 40%: 10% to 40%: 10% to 70%, and the sum of the filling ratios of each stage is 100%; the preferred filling ratios are: 10% to 40%: 10% to 40%: 10% to 40%: 10% to 40%, and the sum of the filling ratios of each stage is 100%.

[0021] Furthermore, the alumina carrier is prepared by molding / modifying hydrated alumina and / or an alumina composition; wherein the hydrated alumina and / or the alumina composition contains tri-coordinated aluminum ions, tetra-coordinated aluminum ions and penta-coordinated aluminum ions.

[0022] Furthermore, the hydrogenation catalyst is preferably a heavy oil hydrogenation catalyst commonly used in the art, wherein, along the flow direction of the reactants, the pore volume of each stage of the hydrogenation catalyst decreases step by step, the pore size decreases step by step, the activity increases step by step, and the particle size decreases step by step, such as a hydrodesulfurization agent, a hydrodecarbonization agent, a hydrodenitrogenation agent, an aromatic saturation agent, and the like.

[0023] Furthermore, in each stage of hydrogenation catalyst, the active metal is selected from at least one of Group VIII and / or Group VIB metal elements, and based on the weight of the hydrogenation catalyst, the active metal is calculated as oxide, the content of Group VIII metal is 0.2wt% to 9.0wt%, preferably 0.5wt% to 9.0wt%, and the content of Group VIB metal is 4wt% to 50wt%, preferably 4wt% to 45wt%.

[0024] Furthermore, in each stage of hydrogenation catalyst, the content of the alumina carrier is 45 wt% to 95 wt%, preferably 50 wt% to 95 wt%, based on the weight of the hydrogenation catalyst.

[0025] Furthermore, in the alumina carrier, the control of the content of different coordinated aluminum mainly depends on the calcination temperature during the preparation of the alumina carrier. Increasing the calcination temperature increases the content of penta-coordinate aluminum, while decreasing the calcination temperature increases the content of tri-coordinate aluminum.

[0026] Furthermore, the content of different coordinated aluminum in the alumina carrier can also be controlled by adjusting the pH value during the preparation process of the alumina carrier.

[0027] Furthermore, in the sulfurized hydrogenation catalyst, the average length of the metal active phase crystals and the average number of crystal layers mainly depend on the hydrogenation catalyst preparation method or the sulfurization method, and the sulfurization method can be wet sulfurization or dry sulfurization.

[0028] Furthermore, the calcination temperature during the preparation of the alumina carrier is 300-1000°C.

[0029] Furthermore, it is preferred that the hydrogenation catalyst grading system includes three-stage sulfided hydrogenation catalysts, and the three-stage sulfided hydrogenation catalysts all contain alumina carriers, namely: alumina carrier I, alumina carrier II and alumina carrier III, wherein the calcination temperature of alumina carrier I is preferably 700-1000°C, and the calcination time is 2-10h; the calcination temperature of alumina carrier II is preferably 500-700°C, and the calcination time is 2-10h; the calcination temperature of alumina carrier III is preferably 300-500°C, and the calcination time is 2-10h.

[0030] In the method of the present invention, the synthesis method of alumina used in the alumina carrier I refers to the reaction for preparing aluminum hydroxide gel, which can be specifically one or more of precipitation method (including acid method and alkali method), hydrolysis method, etc. The precipitation method can be one or more of aluminum sulfate method, carbonization method, aluminum chloride method, aluminum nitrate method, etc.; the hydrolysis method can be the hydrolysis reaction of aluminum-containing compounds, such as the hydrolysis of low-carbon aluminum alcohol and high-carbon aluminum alcohol. The prepared alumina raw material is kneaded and extruded into a plastic body, and finally dried and calcined to obtain the desired alumina carrier precursor, the drying temperature is 100-200°C, the calcination temperature is 700-1000°C, and the calcination time is 2-10h.

[0031] In the method of the present invention, the preparation method of the oxidized hydrogenation catalyst I is as follows: the alumina carrier I is supersaturated with a solution containing active metal components to obtain a catalyst precursor, and the desired oxidized hydrogenation catalyst I is obtained after drying and calcination. The drying temperature is 100°C to 300°C, preferably 200°C to 300°C, and the drying time is 1h to 5h, preferably 4h to 5h; the calcination temperature is 500°C to 600°C, preferably 550°C to 580°C, and the calcination time is 1h to 5h, preferably 4h to 5h; the heating rate is 2 to 5°C / min.

[0032] The preparation method of the sulfided hydrogenation catalyst I is as follows: the oxidized hydrogenation catalyst I is loaded into a sulfidation reactor, and sulfided oil (such as at least one of gasoline, diesel, and wax oil) is introduced therein to wet the catalyst bed; then the bed temperature is adjusted to 150-170°C, and a sulfiding agent (such as at least one of carbon disulfide and dimethyl disulfide) is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 250-270°C at a rate of 2-5°C / h, and the temperature is maintained for 8-10 hours; the catalyst bed temperature is increased to 350-360°C at a rate of 5-10°C / h, and the temperature is maintained for 8-10 hours, thereby obtaining the sulfided hydrogenation catalyst I.

[0033] In the method of the present invention, the synthesis method of alumina used in alumina carrier II refers to the reaction for preparing aluminum hydroxide gel, which can be specifically one or more of precipitation method (including acid method and alkali method), hydrolysis method, etc. The precipitation method can be one or more of aluminum sulfate method, carbonization method, aluminum chloride method, aluminum nitrate method, etc.; the hydrolysis method can be the hydrolysis reaction of aluminum-containing compounds, such as the hydrolysis of low-carbon aluminum alcohol and high-carbon aluminum alcohol. Then the prepared alumina raw material is extruded into a plastic body, and finally dried and calcined to obtain the desired alumina carrier precursor, the drying temperature is 100-200°C, the calcination temperature is 500-700°C, and the calcination time is 2-10h.

[0034] In the method of the present invention, the preparation method of the oxidized hydrogenation catalyst II is as follows: impregnating the alumina carrier II with an organic compound solution; heat treating the obtained carrier loaded with organic compound additives; then loading the obtained carrier loaded with organic matter with active metal components to obtain a catalyst precursor, and drying and calcining to obtain the desired oxidized hydrogenation catalyst II. The organic compound can specifically be a compound containing at least two oxygen atom groups and 2-5 carbon atoms, preferably a compound containing at least two hydroxyl groups and 2-5 carbon atoms. The organic additive includes at least one of alcohols, ethers or sugars, wherein the alcohol can include at least one of ethylene glycol, propylene glycol, glycerol, etc., the ether can include at least one of diethylene glycol, propylene glycol, etc., the sugar includes monosaccharides, and the above organic compounds can be selected from one or more of them. The drying temperature is 100°C to 300°C, preferably 150°C to 200°C, the drying time is 1h to 5h, preferably 2h to 3h; the roasting temperature is 400°C to 500°C, preferably 450°C to 480°C, the roasting time is 1h to 5h, preferably 2h to 3h; the heating rate is 5 to 10°C / min. The amount of the organic compound is 5% to 10% of the weight of the hydrogenation catalyst carrier.

[0035] The preparation method of the sulfided hydrogenation catalyst II is as follows: the oxidized hydrogenation catalyst II is loaded into a sulfidation reactor, and sulfided oil (such as at least one of gasoline, diesel, and wax oil) is introduced therein to wet the catalyst bed; then the bed temperature is adjusted to 150-170°C, and a sulfiding agent (such as at least one of carbon disulfide and dimethyl disulfide) is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 210-230°C at a rate of 5-10°C / h, and the temperature is maintained for 5-7 hours; the catalyst bed temperature is increased to 330-340°C at a rate of 10-15°C / h, and the temperature is maintained for 5-7 hours, to obtain the sulfided hydrogenation catalyst II.

[0036] In the method of the present invention, the synthesis method of alumina used in the alumina carrier III refers to the reaction for preparing aluminum hydroxide gel, which can be specifically one or more of precipitation method (including acid method and alkali method), hydrolysis method, etc. The precipitation method can be one or more of aluminum sulfate method, carbonization method, aluminum chloride method, aluminum nitrate method, etc.; the hydrolysis method can be the hydrolysis reaction of aluminum-containing compounds, such as the hydrolysis of low-carbon aluminum alcohol and high-carbon aluminum alcohol. The prepared alumina raw material is mixed and extruded into a plastic body, and finally dried and calcined to obtain the desired alumina carrier precursor, the drying temperature is 100-200°C, the calcination temperature is 300-500°C, and the calcination time is 2-10h.

[0037] In the method of the present invention, the preparation method of the oxidized hydrogenation catalyst III is as follows: the alumina carrier III is saturated with a solution containing an active metal component and an organic compound to obtain a hydrogenation catalyst precursor, and the desired oxidized hydrogenation catalyst III is obtained after drying. The organic compound can be a compound containing at least two oxygen atom groups and 5-20 carbon atoms, preferably a compound containing at least two hydroxyl groups and 5-20 carbon atoms. The organic additive includes at least one of alcohols, ethers or sugars, wherein the alcohol can include glycerol, etc., the ether can include at least one of triethylene glycol, tributylene glycol or tetraethylene glycol, etc., the sugar includes polysaccharide, and the polysaccharide can include at least one of lactose, maltose or sucrose, and the above organic compounds can be selected from one or more of them. The drying temperature is 100°C to 300°C, preferably 100°C to 150°C, the drying time is 1h to 5h, preferably 1h to 1.5h; the heating rate is 2 to 5°C / min. The amount of the organic compound is 15% to 20% of the weight of the hydrogenation catalyst III carrier.

[0038] The preparation method of the sulfided hydrogenation catalyst III is as follows: the oxidized hydrogenation catalyst III is loaded into a sulfidation reactor, and sulfided oil (such as at least one of gasoline, diesel, and wax oil) is introduced therein to wet the catalyst bed; then the bed temperature is adjusted to 150-170° C., and a sulfiding agent (such as at least one of carbon disulfide and dimethyl disulfide) is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 180-200° C. at a rate of 10-15° C. / h, and the temperature is maintained for 2-4 hours; the catalyst bed temperature is increased to 310-320° C. at a rate of 15-20° C. / h, and the temperature is maintained for 2-4 hours, to obtain the sulfided hydrogenation catalyst III.

[0039] The second aspect of the present invention is to provide an application of the aforementioned hydrogenation catalyst grading method in the hydrogenation treatment of inferior raw materials.

[0040] Furthermore, the inferior raw materials include: heavy inferior raw materials such as gasoline, diesel, wax oil, residual oil, coal tar, coal liquefied oil, etc., especially residual oil raw materials.

[0041] Furthermore, the hydrogenation catalyst grading method of the present invention can be used under any suitable hydroprocessing reaction conditions in the art.

[0042] Furthermore, the hydroprocessing reaction conditions are: average reaction temperature of 200°C to 450°C, preferably 250°C to 430°C; reaction hydrogen partial pressure of 4.0MPa to 20.0MPa, preferably 8.0MPa to 18.0MPa; liquid hourly volume space velocity of 0.15h- 1 ~3.0h- 1 , preferably 0.2h- 1 ~2.0h-1 ; The volume ratio of hydrogen to oil is 300 to 1500, preferably 500 to 1200.

[0043] Compared with the prior art, the method of the present invention has the following advantages:

[0044] In the method of the present invention, along the flow direction of the liquid phase reactant, the modified alumina carrier in the hydrogenation catalyst first used has a higher content of penta-coordinated aluminum ions, a moderate content of tetra-coordinated aluminum ions, and a lower content of tri-coordinated aluminum ions, which enhances the interaction between the metal and the alumina defects and weakens the interaction between hydrogen and the alumina surface, thereby increasing the overflow of hydrogen on the catalyst surface. The overflow hydrogen can enhance the catalytic performance of the catalyst, inhibit the deactivation of the catalyst, and remove more metals such as Ni, Fe, V, etc., reduce the carbon on the surface, and the metal active phase crystal length in the sulfided hydrogenation catalyst is shorter, the number of crystal layers is larger, and the catalyst surface can be significantly reduced. Low steric hindrance effect improves the utilization rate of the active phase; the modified alumina carrier in the hydrogenation catalyst finally used has a lower content of penta-coordinated aluminum ions, a moderate content of tetra-coordinated aluminum ions, and an increased content of tri-coordinated aluminum ions, which weakens the interaction between the metal and alumina defects, increases active sites, and reduces the steric hindrance of the reactants, which is beneficial to the removal of difficult-to-remove impurities such as O, S, and N in small molecules. The metal active phase crystal length in the sulfided hydrogenation catalyst is longer and the number of crystal layers is smaller, which further hydrogenates small molecules with smaller steric hindrance, improves the utilization rate of the active metal, and achieves effective reaction on the reactant molecules. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 The NMR analysis results of the alumina carrier I of the catalyst used in Example 1;

[0046] Figure 2 The NMR analysis results of the alumina carrier II of the catalyst used in Example 1;

[0047] Figure 3 The NMR analysis result of the alumina carrier III of the catalyst used in Example 1;

[0048] Figure 4 This is a transmission electron microscope image of the sulfided hydrogenation catalyst I used in Example 1;

[0049] Figure 5 This is a transmission electron microscope image of the sulfided hydrogenation catalyst II used in Example 1;

[0050] Figure 6 This is a transmission electron microscope image of the sulfided hydrogenation catalyst III used in Example 1. DETAILED DESCRIPTION

[0051] The preparation method of the catalyst of the present invention is described in more detail below through specific examples. The examples are only illustrative of the specific implementation of the method of the present invention and do not constitute a limitation on the scope of protection of the present invention.

[0052] Unless otherwise specified in the present invention, the content of coordinated aluminum ions is molar content.

[0053] In the present invention, a Bruker AVANCE III 500 nuclear magnetic resonance spectrometer is used to determine the type and quantity of aluminum ions. Experimental conditions: BBO normal phase observation broadband probe, H decoupling, deuterium lock channel; standard broadband range: BB = 31P-15N; sensitivity: 367S / N1H NMR, 0.1EB 263S / N 13C NMR, ASTM; resolution: 0.38HZ1 H, 0.1CHCL3, 0.13 13CNMR, ASTM.

[0054] In the method of the present invention, the specific surface area and pore structure of the hydrogenation catalyst are determined by low-temperature liquid nitrogen adsorption method.

[0055] In the method of the present invention, the average length and average number of layers of the metal active phase in the hydrogenation catalyst are statistically analyzed using a transmission electron microscope (TEM), the electron gun type: LaB6 gun; acceleration voltage: 200kV; point resolution: 0.23nm; common accessories: Gatan 832 CCD camera, EDAX EDS spectrometer; single / double tilt sample stage; line resolution: 0.14nm; magnification: 50-1500000. During the test, the length and number of active phase crystals in 100 electron microscope pictures are statistically analyzed and the average value is calculated.

[0056] Example 1

[0057] This embodiment provides a catalyst grading solution for long-term operation of inferior raw materials, that is, loading catalysts in the reactor, and loading sulfided hydrogenation catalyst I, sulfided hydrogenation catalyst II and sulfided hydrogenation catalyst III from top to bottom along the flow direction of liquid reactants, wherein the loading volume ratio of sulfided hydrogenation catalysts I, II and III is 50%:25%:25%.

[0058] The alumina raw material used for the alumina carrier I is prepared by hydrolyzing aluminum isopropoxide, and after being mixed, kneaded and extruded into a plastic body, it is dried at 120°C for 3 hours and calcined at 900°C for 3 hours to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 55%, and the content of tetracoordinate aluminum ions is Ф IV The value is 35%, and the content of tri-coordinated aluminum ions is Ф III The value is 10%.

[0059] The preparation method of the sulfided hydrogenation catalyst I is as follows: the alumina carrier I is supersaturated with an impregnation solution containing Mo and Ni active components to obtain a catalyst precursor, the precursor is dried at 150°C for 4.5 hours, the temperature is increased to 550°C at 2°C / min, and the desired catalyst is obtained after constant temperature calcination for 5 hours. In the prepared catalyst, the mass content of MoO3 is 6.0%, the mass content of NiO is 0.9%, and the content of the alumina carrier is 93.1%; the properties of the catalyst are as follows: the specific surface area is 110m 2 / g, and the pore size is 18.7nm. The catalyst is loaded into a sulfurization reactor, and sulfurized oil wax oil is introduced therein to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 260°C at 5°C / h and kept at a constant temperature for 9 hours; the catalyst bed temperature is increased to 350°C at 10°C / h and kept at a constant temperature for 10 hours to obtain a sulfurized hydrogenation catalyst I. In the sulfurized hydrogenation catalyst I, the average number of active phase lamellae is 8.6, and the average length of the lamellae is 2.4nm.

[0060] The alumina raw material used for the alumina carrier II is prepared by the aluminum sulfate method. Urea is added during the kneading process to extrude into a plastic body, which is then dried at 120°C for 2 hours and calcined at 700°C for 3 hours to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 45%, and the content of tetracoordinate aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 15%.

[0061] The preparation method of sulfided hydrogenation catalyst II is as follows: the alumina carrier II is saturated with a mixed solution containing Mo, Ni active components and propylene glycol (propylene glycol is 6% of the catalyst carrier mass) to obtain a catalyst precursor, which is dried at 150°C for 2.5h, heated to 400°C at 5°C / min, and calcined at a constant temperature for 3.0h to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 13.0%, the mass content of NiO is 2.4%, and the content of alumina carrier is 84.6%; the properties of the catalyst are as follows: the specific surface area is 180m 2 / g, and the pore size is 11.8nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 160°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 220°C at 10°C / h and kept at a constant temperature for 7 hours; the catalyst bed temperature is increased to 330°C at 15°C / h and kept at a constant temperature for 7 hours to obtain a sulfurized hydrogenation catalyst II. In the sulfurized hydrogenation catalyst II, the average number of active phase lamellae is 5.7, and the average length of the lamellae is 4.9nm.

[0062] The alumina raw material used for the alumina carrier III is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours and calcined at 500°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 40%, and the content of tetracoordinate aluminum ions is Ф IV The value is 35%, and the content of tri-coordinated aluminum ions is Ф III The value is 25%.

[0063] The preparation method of the sulfided hydrogenation catalyst III is as follows: the carrier III is saturated with a mixed solution containing Mo, Ni active components and lactose (the amount of lactose is 16% of the catalyst carrier mass) to obtain a catalyst precursor, and the precursor is dried at 100°C for 1 hour to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 22.5%, the mass content of NiO is 3.7%, and the content of alumina carrier is 73.8%; the properties of the catalyst are as follows: the specific surface area is 199m 2 / g, and the pore diameter is 8.1nm. The catalyst is loaded into a sulfurization reactor, and sulfurized gasoline is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 160°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 190°C at 15°C / h and kept at a constant temperature for 4 hours; the catalyst bed temperature is increased to 315°C at 20°C / h and kept at a constant temperature for 3 hours to obtain the sulfurized hydrogenation catalyst III. In the sulfurized hydrogenation catalyst III, the average number of active phase lamellae is 2.4, and the average length of the lamellae is 8.1nm.

[0064] Example 2

[0065] This embodiment provides a catalyst grading solution for long-term operation of inferior raw materials, that is, loading catalysts in the reactor, and loading sulfided hydrogenation catalyst I, sulfided hydrogenation catalyst II and sulfided hydrogenation catalyst III from top to bottom along the flow direction of liquid reactants in the bed, wherein the loading volume ratio of sulfided hydrogenation catalysts I, II and III is 50%:30%:20%.

[0066] The alumina raw material used for the alumina carrier I is prepared by hydrolyzing aluminum isopropoxide, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 3 hours and calcined at 950°C for 4 hours to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 60%, and the content of tetracoordinated aluminum ions is Ф IV The value is 30%, the tri-coordinated aluminum ion content Ф III The value is 10%.

[0067] The preparation method of sulfided hydrogenation catalyst I is as follows: the carrier I is supersaturated with an impregnation solution containing Mo and Ni active components to obtain a catalyst precursor, which is dried at 250°C for 4.5 hours, heated to 500°C at 4°C / min, and calcined at a constant temperature for 4.5 hours to obtain the desired catalyst. The prepared catalyst has a MoO3 mass content of 5.5%, a NiO mass content of 0.8%, and an alumina carrier content of 93.7%. The properties of the catalyst are as follows: the specific surface area is 118m 2 / g, and the pore size is 17.9nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel oil is introduced therein to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 255°C at 3°C / h and kept at a constant temperature for 10 hours; the catalyst bed temperature is increased to 350°C at 5°C / h and kept at a constant temperature for 10 hours to obtain a sulfurized hydrogenation catalyst I. In the sulfurized hydrogenation catalyst I, the average number of active phase lamellae is 9.0, and the average length of the lamellae is 2.1nm.

[0068] The alumina raw material used for the alumina carrier II is prepared by the aluminum sulfate method. After adding ethylenediamine during the kneading process to extrude into a plastic body, it is dried at 120°C for 2 hours and calcined at 600°C for 3 hours to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 50%, the content of tetracoordinated aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 15%.

[0069] The preparation method of sulfided hydrogenation catalyst II is as follows: the carrier II is saturated with a mixed solution containing Mo, Ni active components and ethylene glycol (the amount of ethylene glycol is 10% of the mass of the catalyst carrier) to obtain a catalyst precursor, which is dried at 200°C for 3.0h, heated to 480°C at 10°C / min, and calcined at a constant temperature for 3.0h to obtain the desired catalyst. The prepared catalyst has a MoO3 mass content of 13.2%, a NiO mass content of 2.8%, and an alumina carrier content of 84%. The properties of the catalyst are as follows: the specific surface area is 187m 2 / g, and the pore size is 13.9nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel oil is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 220°C at 8°C / h and kept at a constant temperature for 6 hours; the catalyst bed temperature is increased to 340°C at 11°C / h and kept at a constant temperature for 6 hours to obtain a sulfurized hydrogenation catalyst II. In the sulfurized hydrogenation catalyst II, the average number of active phase lamellae is 6.2, and the average length of the lamellae is 5.8nm.

[0070] The alumina raw material used for the alumina carrier III is prepared by carbonization method, and after being mixed, kneaded and extruded into a plastic body, it is dried at 150°C for 2 hours and calcined at 450°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 45%, and the content of tetracoordinate aluminum ions is Ф IV The value is 35%, and the content of tri-coordinated aluminum ions is Ф III The value is 20%.

[0071] The preparation method of the sulfided hydrogenation catalyst III is as follows: the carrier III is saturated with a mixed solution containing Mo, Ni active components and tributylene glycol (the amount of tributylene glycol is 18% of the mass of the catalyst carrier) to obtain a catalyst precursor, and the precursor is dried at 120°C for 1.0h to obtain the desired catalyst. The prepared catalyst has a MoO3 mass content of 23.5%, a NiO mass content of 3.8%, and an alumina carrier content of 72.7%; the properties of the catalyst are as follows: the specific surface area is 210m 2 / g, and the pore diameter is 10.9nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 190°C at 10°C / h and kept at a constant temperature for 3 hours; the catalyst bed temperature is increased to 310°C at 17°C / h and kept at a constant temperature for 3 hours to obtain the sulfurized hydrogenation catalyst III. In the sulfurized hydrogenation catalyst III, the average number of active phase lamellae is 3.0, and the average length of the lamellae is 7.9nm.

[0072] Example 3

[0073] This embodiment provides a catalyst grading solution for long-term operation of inferior raw materials, that is, loading catalysts in the reactor, and loading sulfided hydrogenation catalyst I, sulfided hydrogenation catalyst II and sulfided hydrogenation catalyst III from top to bottom along the flow direction of liquid reactants, wherein the loading volume ratio of sulfided hydrogenation catalysts I, II and III is 15%:25%:60%.

[0074] The alumina raw material used for the alumina carrier I is prepared by hydrolyzing aluminum isopropoxide, and after being mixed and kneaded into a plastic body, it is dried at 200°C for 3 hours and calcined at 800°C for 3 hours to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 50%, the content of tetracoordinated aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 10%.

[0075] The preparation method of sulfided hydrogenation catalyst I is as follows: the carrier I is supersaturated with an impregnation solution containing Mo and Ni active components to obtain a catalyst precursor, which is dried at 250°C for 4.5 hours, heated to 500°C at 4°C / min, and calcined at a constant temperature for 4.5 hours to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 4.2%, the mass content of NiO is 0.8%, and the content of alumina carrier is 95%; the properties of the catalyst are as follows: the specific surface area is 111m 2 / g, and the pore size is 21.7nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel oil is introduced therein to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 255°C at 3°C / h and kept at a constant temperature for 10 hours; the catalyst bed temperature is increased to 350°C at 5°C / h and kept at a constant temperature for 10 hours to obtain a sulfurized hydrogenation catalyst I. In the sulfurized hydrogenation catalyst I, the average number of active phase lamellae is 7.9, and the average length of the lamellae is 2.5nm.

[0076] The alumina raw material used for the alumina carrier II was prepared by the aluminum sulfate method. After adding diethylene glycol during the kneading process, it was extruded into a plastic body, dried at 120°C for 2h, and calcined at 700°C for 3h to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II was Φ V The value is 45%, and the content of tetracoordinate aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 15%.

[0077] The preparation method of sulfided hydrogenation catalyst II is as follows: the carrier II is saturated with a mixed solution containing active components of Mo and Ni and ethylene glycol (the amount of ethylene glycol is 10% of the mass of the catalyst carrier) to obtain a catalyst precursor, which is dried at 200°C for 3.0h, heated to 480°C at 10°C / min, and calcined at a constant temperature for 3.0h to obtain the desired catalyst. The prepared catalyst has a MoO3 mass content of 11.3%, a NiO mass content of 1.8%, and an alumina carrier content of 86.9%; the properties of the catalyst are as follows: the specific surface area is 154m 2 / g, and the pore size is 15.3nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 220°C at 8°C / h and kept at a constant temperature for 6 hours; the catalyst bed temperature is increased to 340°C at 11°C / h and kept at a constant temperature for 6 hours to obtain the sulfurized hydrogenation catalyst II. In the sulfurized hydrogenation catalyst II, the average number of active phase lamellae is 4.8, and the average length of the lamellae is 5.5nm.

[0078] The alumina raw material used for the alumina carrier III is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours and calcined at 500°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 40%, and the content of tetracoordinate aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 20%.

[0079] The preparation method of sulfided hydrogenation catalyst III is as follows: the carrier III is saturated with a mixed solution containing active components of Mo and Ni and lactose (the amount of lactose is 17% of the mass of the catalyst carrier) to obtain a catalyst precursor, and the precursor is dried at 120°C for 1.5 hours to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 22.3%, the mass content of NiO is 3.9%, and the content of alumina carrier is 73.8%; the properties of the catalyst are as follows: the specific surface area is 222m 2 / g, and the pore size is 9.0nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 160°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 200°C at 15°C / h and kept at a constant temperature for 4.5 hours; the catalyst bed temperature is increased to 310°C at 20°C / h and kept at a constant temperature for 2 hours to obtain a sulfurized hydrogenation catalyst III. In the sulfurized hydrogenation catalyst III, the average number of active phase lamellae is 2.0, and the average length of the lamellae is 7.9nm.

[0080] Comparative Example 1

[0081] This example provides a catalyst grading solution for long-term operation with inferior raw materials, i.e., loading catalysts in the reactor, with the bed layer loaded with sulfided hydrogenation catalyst I, sulfided hydrogenation catalyst II and sulfided hydrogenation catalyst III from top to bottom, wherein the loading volume ratio of sulfided hydrogenation catalysts I, II and III is 15%:25%:60%.

[0082] The alumina raw material used for the alumina carrier I is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours and calcined at 500°C for 3 hours to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier I is Φ V The value is 40%, and the content of tetracoordinate aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 20%.

[0083] The preparation method of sulfided hydrogenation catalyst I is as follows: the carrier I is supersaturated with an impregnation solution containing Mo and Ni active components to obtain a catalyst precursor, which is dried at 250°C for 4.5 hours, heated to 500°C at 4°C / min, and calcined at a constant temperature for 4.5 hours to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 4.2%, the mass content of NiO is 0.9%, and the content of alumina carrier is 94.9%. The properties of the catalyst are as follows: the specific surface area is 112m 2 / g, and the pore size is 21.7nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel oil is introduced therein to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 255°C at 3°C / h and kept at a constant temperature for 10 hours; the catalyst bed temperature is increased to 350°C at 5°C / h and kept at a constant temperature for 10 hours to obtain a sulfurized hydrogenation catalyst I. In the sulfurized hydrogenation catalyst I, the average number of active phase lamellae is 7.9, and the average length of the lamellae is 2.5nm.

[0084] The alumina raw material used for the alumina carrier II was prepared by the aluminum sulfate method. After adding diethylene glycol during the kneading process, it was extruded into a plastic body, dried at 120°C for 2h, and calcined at 700°C for 3h to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II was Φ V The value is 45%, and the content of tetracoordinate aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 15%.

[0085] The preparation method of sulfided hydrogenation catalyst II is as follows: the carrier II is saturated with a mixed solution containing Mo, Ni active components and ethylene glycol (ethylene glycol is 10% of the catalyst carrier mass) to obtain a catalyst precursor, which is dried at 200°C for 3.0h, heated to 480°C at 10°C / min, and calcined at a constant temperature for 3.0h to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 11.3%, the mass content of NiO is 1.8%, and the content of alumina carrier is 86.9%. The properties of the catalyst are as follows: the specific surface area is 159m 2 / g, and the pore size is 16.2nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 220°C at 8°C / h and kept at a constant temperature for 6 hours; the catalyst bed temperature is increased to 340°C at 11°C / h and kept at a constant temperature for 6 hours to obtain a sulfurized hydrogenation catalyst II. In the sulfurized hydrogenation catalyst II, the average number of active phase lamellae is 4.8, and the average length of the lamellae is 5.5nm.

[0086] The alumina raw material used for the alumina carrier III is prepared by hydrolyzing aluminum isopropoxide, and after being mixed and kneaded into a plastic body, it is dried at 200°C for 3 hours and calcined at 800°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared alumina carrier III is Φ V The value is 50%, the content of tetracoordinated aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 10%.

[0087] The preparation method of sulfided hydrogenation catalyst III is as follows: the carrier III is saturated with a mixed solution containing Mo, Ni active components and lactose (the amount of lactose is 17% of the catalyst carrier mass) to obtain a catalyst precursor, and the precursor is dried at 120°C for 1.5 hours to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 21.3%, the mass content of NiO is 3.7%, and the content of alumina carrier is 75%. The properties of the catalyst are as follows: the specific surface area is 221m 2 / g, and the pore size is 10.2nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 160°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 200°C at 15°C / h and kept at a constant temperature for 4.5 hours; the catalyst bed temperature is increased to 310°C at 20°C / h and kept at a constant temperature for 2 hours to obtain a sulfurized hydrogenation catalyst III. In the sulfurized hydrogenation catalyst III, the average number of active phase lamellae is 2.0, and the average length of the lamellae is 7.9nm.

[0088] Comparative Example 2

[0089] This example provides a catalyst grading solution for long-term operation with inferior raw materials, i.e., loading catalysts in the reactor, with the bed layer loaded with sulfided hydrogenation catalyst I, sulfided hydrogenation catalyst II and sulfided hydrogenation catalyst III from top to bottom, wherein the loading volume ratio of sulfided hydrogenation catalysts I, II and III is 15%:25%:60%.

[0090] The alumina raw material used for the alumina carrier I is prepared by hydrolyzing aluminum isopropoxide, and after being mixed and kneaded into a plastic body, it is dried at 200°C for 3 hours and calcined at 800°C for 3 hours to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 50%, the content of tetracoordinated aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 10%.

[0091] The preparation method of sulfided hydrogenation catalyst I is as follows: the carrier I is supersaturated with an impregnation solution containing Mo and Ni active components to obtain a catalyst precursor, which is dried at 250°C for 4.5 hours, heated to 500°C at 4°C / min, and calcined at a constant temperature for 4.5 hours to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 4.4%, the mass content of NiO is 0.9%, and the content of alumina carrier is 94.7%. The properties of the catalyst are as follows: the specific surface area is 121m 2 / g, and the pore size is 22.7nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel oil is introduced therein to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 255°C at 3°C / h and kept at a constant temperature for 10 hours; the catalyst bed temperature is increased to 350°C at 5°C / h and kept at a constant temperature for 10 hours to obtain a sulfurized hydrogenation catalyst I. In the sulfurized hydrogenation catalyst I, the average number of active phase lamellae is 7.9, and the average length of the lamellae is 2.5nm.

[0092] The alumina raw material used for the alumina carrier II was prepared by the aluminum sulfate method. After adding diethylene glycol during the kneading process, it was extruded into a plastic body, dried at 120°C for 2h, and calcined at 700°C for 3h to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II was Φ V The value is 50%, the content of tetracoordinated aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 10%.

[0093] The preparation method of sulfided hydrogenation catalyst II is as follows: the carrier II is saturated with a mixed solution containing Mo, Ni active components and ethylene glycol (ethylene glycol is 10% of the catalyst carrier mass) to obtain a catalyst precursor, which is dried at 200°C for 3.0h, heated to 480°C at 10°C / min, and calcined at a constant temperature for 3.0h to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 11.3%, the mass content of NiO is 1.8%, and the content of alumina carrier is 86.9%. The properties of the catalyst are as follows: the specific surface area is 159m 2 / g, and the pore size is 15.7nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 220°C at 8°C / h and kept at a constant temperature for 6 hours; the catalyst bed temperature is increased to 340°C at 11°C / h and kept at a constant temperature for 6 hours to obtain a sulfurized hydrogenation catalyst II. In the sulfurized hydrogenation catalyst II, the average number of active phase lamellae is 4.8, and the average length of the lamellae is 5.5nm.

[0094] The alumina raw material used for the alumina carrier III is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours and calcined at 500°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 50%, the content of tetracoordinated aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 10%.

[0095] The preparation method of sulfided hydrogenation catalyst III is as follows: the carrier III is saturated with a mixed solution containing Mo, Ni active components and lactose (the amount of lactose is 17% of the catalyst carrier mass) to obtain a catalyst precursor, and the precursor is dried at 120°C for 1.5 hours to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 22.3%, the mass content of NiO is 3.4%, and the content of alumina carrier is 74.3%. The properties of the catalyst are as follows: the specific surface area is 221m 2 / g, and the pore size is 9.8nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel oil is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 160°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 200°C at 15°C / h and kept at a constant temperature for 4.5 hours; the catalyst bed temperature is increased to 310°C at 20°C / h and kept at a constant temperature for 2 hours to obtain the sulfurized hydrogenation catalyst III. In the sulfurized hydrogenation catalyst III, the average number of active phase lamellae is 2.0, and the average length of the lamellae is 7.9nm.

[0096] Comparative Example 3

[0097] This example provides a catalyst grading solution for long-term operation with inferior raw materials, i.e., loading catalysts in the reactor, with the bed layer loaded with sulfided hydrogenation catalyst I, sulfided hydrogenation catalyst II and sulfided hydrogenation catalyst III from top to bottom, wherein the loading volume ratio of sulfided hydrogenation catalysts I, II and III is 15%:25%:60%.

[0098] The alumina raw material used for the alumina carrier I is prepared by hydrolyzing aluminum isopropoxide, and after being mixed and kneaded into a plastic body, it is dried at 200°C for 3 hours and calcined at 800°C for 3 hours to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 50%, the content of tetracoordinated aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 10%.

[0099] The preparation method of hydrogenation catalyst I is as follows: the carrier I is supersaturated with an impregnation solution containing Mo and Ni active components to obtain a catalyst precursor, which is dried at 250°C for 4.5 hours, heated to 500°C at 4°C / min, and calcined at a constant temperature for 4.5 hours to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 4.2%, the mass content of NiO is 0.8%, and the content of alumina carrier is 95%. The properties of the catalyst are as follows: the specific surface area is 102m 2 / g, and the pore size is 21.7nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel oil is introduced therein to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 255°C at 3°C / h and kept at a constant temperature for 10 hours; the catalyst bed temperature is increased to 350°C at 5°C / h and kept at a constant temperature for 10 hours to obtain a sulfurized hydrogenation catalyst I. In the sulfurized hydrogenation catalyst I, the average number of active phase lamellae is 2.2, and the average length of the lamellae is 7.8nm.

[0100] The alumina raw material used for the alumina carrier II was prepared by the aluminum sulfate method. After adding diethylene glycol during the kneading process, it was extruded into a plastic body, dried at 120°C for 2h, and calcined at 700°C for 3h to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II was Φ V The value is 45%, and the content of tetracoordinate aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 15%.

[0101] The preparation method of sulfided hydrogenation catalyst II is as follows: the carrier II is supersaturated with an impregnation solution containing Mo and Ni active components to obtain a catalyst precursor, which is dried at 250°C for 4.5 hours, heated to 500°C at 4°C / min, and calcined at a constant temperature for 4.5 hours to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 11.3%, the mass content of NiO is 1.8%, and the content of alumina carrier is 86.9%. The properties of the catalyst are as follows: the specific surface area is 157m 2 / g, and the pore size is 16.2nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 255°C at 3°C / h and kept at a constant temperature for 10 hours; the catalyst bed temperature is increased to 350°C at 5°C / h and kept at a constant temperature for 10 hours to obtain a sulfurized hydrogenation catalyst II. In the sulfurized hydrogenation catalyst II, the average number of active phase lamellae is 2.2, and the average length of the lamellae is 8.0nm.

[0102] The alumina raw material used for the alumina carrier III is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours and calcined at 500°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 40%, and the content of tetracoordinate aluminum ions is Ф IV The value is 40%, and the content of tri-coordinated aluminum ions is Ф III The value is 20%.

[0103] The preparation method of sulfided hydrogenation catalyst III is as follows: the carrier III is supersaturated with an impregnation solution containing Mo and Ni active components to obtain a catalyst precursor, which is dried at 250°C for 4.5 hours, heated to 500°C at 4°C / min, and calcined at a constant temperature for 4.5 hours to obtain the desired catalyst. The mass content of MoO3 in the prepared catalyst is 22.3%, the mass content of NiO is 3.9%, and the content of alumina carrier is 73.8%. The properties of the catalyst are as follows: the specific surface area is 221m 2 / g, and the pore size is 10.2nm. The catalyst is loaded into a sulfurization reactor, and sulfurized diesel is introduced into it to wet the catalyst bed; then the bed temperature is adjusted to 170°C, and the sulfurizing agent carbon disulfide is injected; after hydrogen sulfide penetrates the catalyst bed, the catalyst bed temperature is increased to 255°C at 3°C / h and kept at a constant temperature for 10 hours; the catalyst bed temperature is increased to 350°C at 5°C / h and kept at a constant temperature for 10 hours to obtain the sulfurized hydrogenation catalyst III. In the sulfurized hydrogenation catalyst III, the average number of active phase lamellae is 2.0, and the average length of the lamellae is 7.9nm.

[0104] Example 4

[0105] This example is a comparative test of the activity and stability of the catalyst combination system of Examples 1, 2, 3 and Comparative Examples 1, 2, 3 on a 100mL fixed bed small hydrogenation device, and the feeding method adopts upper feeding. The properties of the evaluated raw oil are shown in Table 1; the evaluation conditions are shown in Table 2; the catalyst combination scheme is shown in Table 3; and the evaluation results of the catalyst combination scheme are shown in Table 4.

[0106] Table 1 Raw oil properties

[0107] Crude oil Residue <![CDATA[Density (20 °C), g·cm- 3 > 1.034 Carbon residue, wt% 20.11 S, wt% 5.22 <![CDATA[Ni+V,μg·g- 1 ]]> 178.5

[0108] Table 2 Evaluation process conditions

[0109] Reaction temperature, °C 380 Reaction hydrogen partial pressure, MPa 15.0 <![CDATA[Liquid hourly space velocity, h- 1 > 0.7 Hydrogen to oil volume ratio 800:1

[0110] Table 3 Evaluation results of various catalyst combinations

[0111]

[0112] The above describes the specific implementation of the present invention in detail, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the various technical features being combined in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A hydrogenation catalyst grading method, characterized in that: It includes a graded system consisting of n-level sulfided hydrogenation catalysts, wherein n≥3, each level of hydrogenation catalyst comprises an alumina carrier and a metal active component, wherein the alumina carrier contains three types of aluminum ions: tri-coordinated aluminum ions Al 3+ Ⅲ , four-coordinated aluminum ion Al 3+ Ⅳ and pentacoordinated aluminum ion Al 3 + Ⅴ , the content of pentacoordinated aluminum ions φ in the flow direction of liquid phase reactants of each hydrogenation catalyst is based on the total amount of three ligands of aluminum in the alumina carrier. V The content of tri-coordinated aluminum ions decreases gradually, with a decrease of 5 to 15 percentage points. III It increases step by step, with the increment ranging from 1 to 10 percentage points. For each level of sulfided hydrogenation catalyst along the flow direction of the liquid reactants, the average length of the metal active phase lamellae increases step by step, and the average number of lamellae decreases step by step.

2. The grading method according to claim 1, characterized in that: The catalyst grading method comprises a grading system composed of n-grade sulfided hydrogenation catalysts, wherein n is 3 or 4.

3. The grading method according to claim 1, characterized in that: Along the flow direction of the liquid reactants, in each level of sulfided hydrogenation catalyst, the average length of the metal active phase crystal is 1~9nm, increasing by 1~5nm step by step, and the average number of metal active phase crystal layers is 1~9, decreasing by 1~5 step by step.

4. The grading method according to claim 1, characterized in that: Along the flow direction of the liquid reactants, in each level of sulfided hydrogenation catalyst, the average length of the metal active phase crystal is 1~9nm, increasing by 2~4nm step by step, and the average number of metal active phase crystal layers is 1~9, decreasing by 2~4 step by step.

5. The grading method according to claim 1, characterized in that: In the alumina carrier of each level of hydrogenation catalyst, the total content of three ligand aluminum is taken as the basis, and the content of pentacoordinate aluminum ion is φ V 40%~60%, the content of tetracoordinated aluminum ions φ IV 30%~50%, tri-coordinated aluminum ion content φ III It is 10%~30%.

6. The grading method according to claim 1, characterized in that: In the alumina carrier of the same grade catalyst, the content of pentacoordinated aluminum ions is V ≥Tetracoordinated aluminum ion contentφ IV ≥Tricoordinated aluminum ion contentφ III .

7. The grading method according to claim 1 or 6, characterized in that: In the alumina carrier of the same grade of catalyst, the difference between the content of penta-coordinated aluminum ions and the content of tri-coordinated aluminum ions is 15%~50%.

8. The grading method according to claim 1, characterized in that: The graded system includes three sulfide hydrogenation catalysts. Based on the total volume of the catalyst in the reactor, the three-stage filling ratios along the flow direction of the liquid reactants are 10%~90%: 5%~40%: 5%~80%, and the sum of the filling ratios of each stage is 100%.

9. The grading method according to claim 1, characterized in that: The graded system includes four sulfide hydrogenation catalysts. Based on the total volume of the catalyst in the reactor, the four-stage filling ratios along the flow direction of the liquid reactants are: 10%~70%: 10%~40%: 10%~40%: 10%~70%, and the sum of the filling ratios of each stage is 100%.

10. The grading method according to claim 1, characterized in that: The graded system includes four sulfide hydrogenation catalysts. Based on the total volume of the catalyst in the reactor, the four-stage filling ratios along the flow direction of the liquid reactants are: 10%~40%: 10%~40%: 10%~40%: 10%~40%, and the sum of the filling ratios of each stage is 100%.

11. The grading method according to claim 1, characterized in that: In each stage of hydrogenation catalyst, the active metal is selected from at least one of Group VIII and / or Group VIB metal elements. Based on the weight of the hydrogenation catalyst, the active metal is calculated as oxide, the content of Group VIII metal is 0.2wt%~9.0wt%, and the content of Group VIB metal is 4wt%~50wt%.

12. The grading method according to claim 1, characterized in that: In each stage of hydrogenation catalyst, the active metal is selected from at least one of Group VIII and / or Group VIB metal elements. Based on the weight of the hydrogenation catalyst, the active metal is calculated as oxide, the content of Group VIII metal is 0.5wt%~9.0wt%, and the content of Group VIB metal is 4wt%~45wt%.

13. The grading method according to claim 1, characterized in that: In each level of hydrogenation catalyst, the content of the alumina carrier is 45wt%~95wt% based on the weight of the hydrogenation catalyst.

14. The grading method according to claim 1, characterized in that: In each level of hydrogenation catalyst, the content of the alumina carrier is 50wt%~90wt% based on the weight of the hydrogenation catalyst.

15. Use of the catalyst grading method according to any one of claims 1 to 14 in the hydroprocessing of inferior raw materials.

16. The use according to claim 15, characterized in that The reaction conditions of the hydrotreatment are: average reaction temperature of 200°C to 450°C; reaction hydrogen partial pressure of 4.0MPa to 20.0MPa; liquid hourly volume space velocity of 0.15h -1 ~3.0h -1 ; The volume ratio of hydrogen to oil is 300~1500.

17. The use according to claim 15, characterized in that: The reaction conditions of the hydrotreatment are: average reaction temperature of 250°C to 430°C; reaction hydrogen partial pressure of 8.0MPa to 18.0MPa; liquid hourly volume space velocity of 0.2h -1 ~2.0h -1 ; The volume ratio of hydrogen to oil is 500~1200.