A nitrogen-doped copper manganate / carbon composite material and its preparation method and application
The nitrogen-doped copper manganate/carbon composite material is prepared by a one-step calcination method, which solves the problems of low BPA removal efficiency and difficulty in catalyst recycling in the existing technology, achieves efficient activation of persulfate, and completely degrades BPA in a short time, and Maintaining the characteristics of high efficiency and environmental protection.
Patent Information
- Application Number
- CN202310400195.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-11
AI Technical Summary
When existing technologies remove bisphenol A (BPA) pollutants, the biodegradation method is inefficient and the physical adsorption method has problems with pollutant transfer. The efficiency of activated persulfate in advanced oxidation technology is low and the catalyst is difficult to recycle and is heterogeneous. Transition metal oxides have low activation efficiency and are not environmentally friendly.
Nitrogen-doped copper manganate/carbon composite materials are prepared through a one-step calcination method. Urea is used to provide a nitrogen source and ammonia gas decomposed at high temperature is used to introduce heteroatoms, generate oxygen vacancies, improve the activation efficiency of persulfate, and improve the structure of the composite material. Degradation rate and mineralization degree of BPA.
It achieves efficient activation of persulfate, completely degrades BPA in a short time (within 9 minutes), and reaches 98% deep mineralization, and the composite material can be reused. The BPA degradation rate still reaches more than 85% during the fourth activation. Stable structure, efficient and environmentally friendly.
Smart Images

Figure CN116440938B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of water pollution treatment, and in particular to a nitrogen-doped copper manganate / carbon composite material and a preparation method and application thereof. Background Art
[0002] Bisphenol A (BPA), as a representative of endocrine disrupting chemicals (EDCs), has been detected in sediments, surface water, and drinking water. Even at low exposure levels, BPA has strong estrogenic effects, which may cause endocrine disorders and premature puberty in infants, thus threatening human health. Therefore, the development of efficient BPA treatment technology remains an urgent and challenging task.
[0003] At present, there are three main methods for removing BPA: biodegradation, physical adsorption and advanced oxidation technology (AOP). The biodegradation method has broad prospects for treating BPA, but it also has many disadvantages, such as high requirements for bacterial strains. At the same time, because BPA may be toxic to microorganisms, its biodegradation takes a long time, which limits its practical application. Although the physical adsorption method can quickly and effectively remove BPA, the adsorption method does not remove BPA by degradation, but transfers BPA from the aqueous phase to the solid phase, which is only a secondary transfer of pollutants. Advanced oxidation technology based on sulfate free radicals (SR-AOPs) has become a hot topic among researchers due to its wide working pH range, high efficiency, and environmental friendliness. Permonosulfate (PMS) and peroxydisulfate (PDS) are sulfate free radicals (SO4 ·- ), PMS is more easily activated due to the asymmetry of its molecular structure, thereby inducing the cleavage of the OO bond to generate SO4 ·- and ·OH. However, since the persulfate ions produced by persulfate have good chemical stability in water and very low reactivity with organic pollutants, external energy or catalysts are required to activate persulfate to degrade BPA by generating active oxygen. Methods for activating persulfate include ultraviolet light, thermal energy and transition metals. Compared with ultraviolet light and thermal energy, transition metals and metal oxides have been widely used to activate PMS to degrade organic pollutants because they do not require additional energy input and the catalysts can be recycled and reused. However, in homogeneous systems, they are greatly limited by the toxicity of metal ions, the difficulty of recycling, and the narrow pH application range. Heterogeneous transition metal oxides such as single metal oxides (Co3O4, Fe2O3, MnO2) or multi-metal oxides (FeCo2O4, CuFe2O4, FeNi2O4) have attracted much attention because they can solve the above problems, but they still have relatively low activation efficiency, poor recyclability, and environmental problems. Summary of the invention
[0004] In view of the above shortcomings of the prior art, one of the objectives of the present invention is to provide a method for preparing a nitrogen-doped copper manganate / carbon composite material.
[0005] The above object of the present invention is achieved through the following technical solutions:
[0006] A method for preparing a nitrogen-doped copper manganate / carbon composite material comprises the following steps:
[0007] S1. The urea, organic acid, manganese salt and copper salt are mixed and ground to obtain a mixture;
[0008] S2. calcining the mixture obtained in step S1 at 500-600° C. for 1-4 hours to obtain the nitrogen-doped copper manganate / carbon composite material.
[0009] The invention prepares the nitrogen-doped copper manganate / carbon composite material by a one-step calcination method, the method is simple and suitable for large-scale production.
[0010] In the preparation method of the present invention, urea provides a nitrogen source and decomposes ammonia at a high temperature. The generated ammonia coordinates with a transition metal, introduces heteroatoms, and generates oxygen vacancies. Therefore, the obtained nitrogen-doped copper manganate / carbon composite material has a large specific surface area, is rich in oxygen vacancies, has abundant active sites, can efficiently activate persulfate to generate sulfate radicals, and greatly improves the degradation rate and mineralization degree of persulfate to BPA. At the same time, the composite material has a structure of being doped with nitrogen and composited with carbon, which can further improve the degradation rate of BPA.
[0011] Preferably, in step S1, the organic acid includes at least one of oxalic acid, citric acid and tartaric acid.
[0012] Preferably, in step S1, the manganese salt includes one of manganese sulfate, manganese chloride and manganese nitrate, and the copper salt includes one of copper sulfate, copper chloride and copper nitrate.
[0013] Preferably, in step S1, the molar ratio of the manganese salt to the copper salt is (1-5): 1. Further preferably, the molar ratio of the manganese salt to the copper salt is 2:1.
[0014] Preferably, in step S1, the mass molar ratio of the total amount of urea, organic acid, manganese salt and copper salt is (0.5-10) g: (1-4) g: 0.6 mmol.
[0015] Preferably, in step S2, the calcination temperature is 500° C. and the calcination time is 2 h.
[0016] Another object of the present invention is to provide a nitrogen-doped copper manganate / carbon composite material for activating persulfate, which is prepared by the preparation method.
[0017] Another object of the present invention is to provide an application of the nitrogen-doped copper manganate / carbon composite material of the activated persulfate in the degradation of organic pollutants, the method being as follows: adding the nitrogen-doped copper manganate / carbon composite material of the activated persulfate to organic pollutants, placing it in a dark place to reach adsorption equilibrium, and then adding a persulfate solution to carry out a degradation reaction.
[0018] Preferably, the organic pollutant is a BPA solution, and the persulfate is a peroxymonosulfate or a peroxydisulfate.
[0019] Compared with the prior art, the present invention is beneficial in that:
[0020] (1) In the preparation method of the present invention, urea provides a nitrogen source and decomposes ammonia at a high temperature. The generated ammonia coordinates with the transition metal, introduces heteroatoms, and generates oxygen vacancies. Therefore, the obtained nitrogen-doped copper manganate / carbon composite material is rich in oxygen vacancies, provides more active sites, and can efficiently activate persulfate, greatly improving the degradation rate and mineralization degree of persulfate to BPA. At the same time, the composite material has a structure of being doped with nitrogen and composited with carbon, which can further improve the degradation rate of BPA.
[0021] (2) The composite material prepared by the present invention has an excellent catalytic effect on PMS as a persulfate catalyst, and can completely degrade BPA and achieve deep mineralization (>98%) within 9 minutes; and has good reusability. After the persulfate is activated for the fourth time, the degradation rate of BPA can still reach more than 85%.
[0022] (3) The composite material prepared by the present invention has a stable structure, high efficiency and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a SEM image of the composite material prepared in Example 1;
[0024] Figure 2 XRD pattern of the composite material prepared in Example 1;
[0025] Figure 3 The XPS peak diagram of O1s and the ESR spectrum of oxygen vacancies in the composite material prepared in Example 1;
[0026] Figure 4 This is a diagram of BPA degradation efficiency of the composite materials prepared in Example 1 and Comparative Examples 1 to 3;
[0027] Figure 5 This is a diagram showing the BPA mineralization effect of the composite material prepared in Example 1;
[0028] Figure 6 This is the BPA degradation efficiency diagram under different manganese-copper ratios;
[0029] Figure 7 This is a graph showing the BPA degradation efficiency of the composite material prepared in Example 1 after being reused four times. DETAILED DESCRIPTION
[0030] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] This embodiment provides a method for preparing a nitrogen-doped copper manganate / carbon composite material, which specifically includes the following steps:
[0033] S1. 10 g urea, 4 g oxalic acid, 0.4 mmol manganese sulfate monohydrate and 0.2 mmol copper sulfate pentahydrate were poured into a mortar and mixed and ground for 10 min until the materials were uniformly mixed to obtain a mixture;
[0034] S2. The mixture obtained in step S1 is transferred to a covered crucible, and then the crucible is placed in a muffle furnace, and the temperature is increased to 500° C. at a rate of 5° C. / min and calcined for 2 h to obtain a nitrogen-doped copper manganate / carbon composite material.
[0035] Figure 1 This is the SEM image of the nitrogen-doped copper manganate / carbon composite material prepared in Example 1. Figure 1 It can be seen that the composite material is composed of numerous nanospheres, which are highly cross-linked into a porous structure. Figure 2 is the XRD pattern of nitrogen-doped copper manganate / carbon composite material. Figure 2 It can be seen that nitrogen-doped copper manganate / carbon composites were successfully synthesized. Figure 3 (a) and (b) are the XPS peak diagram of O1s and the ESR spectrum of oxygen vacancies in nitrogen-doped copper manganate / carbon composites, respectively. Figure 3 (a) It can be seen that O 1s is divided into four peaks, namely lattice oxygen (529.9 eV), oxygen vacancies (530.5 eV), surface adsorbed oxygen (531.5 eV) and surface adsorbed water or hydroxyl functional groups (533.2 eV). Figure 3 (b) The generation of strong oxygen vacancy signals can be seen. These results confirm that the prepared composite structure is rich in oxygen vacancies.
[0036] Example 2
[0037] This embodiment provides a method for preparing a nitrogen-doped copper manganate / carbon composite material, which specifically comprises the following steps:
[0038] S1. 5 g urea, 2 g citric acid, 0.4 mmol manganese chloride tetrahydrate and 0.2 mmol copper chloride dihydrate were poured into a mortar and mixed and ground for 10 min until the materials were uniformly mixed to obtain a mixture;
[0039] S2. The mixture obtained in step S1 is transferred to a covered crucible, and then the crucible is placed in a muffle furnace, and the temperature is increased to 550° C. at a rate of 5° C. / min and calcined for 3 h to obtain a nitrogen-doped copper manganate / carbon composite material.
[0040] Example 3
[0041] This embodiment provides a method for preparing a nitrogen-doped copper manganate / carbon composite material, which specifically comprises the following steps:
[0042] S1. 1 g of urea, 1 g of citric acid, 0.4 mmol of manganese nitrate tetrahydrate and 0.2 mmol of copper nitrate trihydrate were poured into a mortar and mixed and ground for 10 min until the materials were uniformly mixed to obtain a mixture;
[0043] S2. The mixture obtained in step S1 is transferred to a covered crucible, and then the crucible is placed in a muffle furnace, and the temperature is increased to 600° C. at a rate of 8° C. / min and calcined for 1 hour to obtain a nitrogen-doped copper manganate / carbon composite material.
[0044] Examples 4-7 Effect of the molar ratio of manganese salt to copper salt on the catalytic performance of the composite material
[0045] The method is basically the same as Example 1, except that the dosage of manganese sulfate monohydrate and copper sulfate pentahydrate is different, as shown in Table 1.
[0046] Table 1 Effect of the dosage of manganese salt and copper salt
[0047] Example Manganese sulfate monohydrate / mmol Copper sulfate pentahydrate / mmol BPA degradation rate (after 9 minutes) Example 1 0.4 0.2 100% Example 4 0.3 0.3 99% Example 5 0.2 0.4 87% Example 6 0.5 0.1 99% Example 7 0.1 0.5 68%
[0048] As can be seen from Table 1, when the molar ratio of manganese salt to copper salt is 2:1, the nitrogen-doped copper manganate / carbon composite material has the best catalytic effect on PMS, and BPA can be completely degraded within 9 minutes.
[0049] Comparative Example 1
[0050] This comparative example provides a method for preparing a nitrogen-doped manganese tetraoxide / carbon composite material, which specifically comprises the following steps:
[0051] S1. 10 g urea, 4 g oxalic acid, and 0.6 mmol manganese sulfate monohydrate were poured into a mortar and mixed and ground for 10 min until the materials were uniformly mixed to obtain a mixture;
[0052] S2. The mixture obtained in step S1 is transferred to a covered crucible, and then the crucible is placed in a muffle furnace, and the temperature is increased to 500° C. at a rate of 5° C. / min and calcined for 2 h to obtain a nitrogen-doped manganese tetraoxide / carbon composite material.
[0053] That is, Comparative Example 1 is substantially the same as Example 1, except that it does not contain copper sulfate pentahydrate.
[0054] Comparative Example 2
[0055] This comparative example provides a method for preparing a nitrogen-doped copper oxide / carbon composite material, which specifically comprises the following steps:
[0056] S1. 10 g urea, 4 g oxalic acid and 0.6 mmol copper sulfate pentahydrate were poured into a mortar and mixed and ground for 10 min until the materials were uniformly mixed to obtain a mixture;
[0057] S2. The mixture obtained in step S1 is transferred to a covered crucible, and then the crucible is placed in a muffle furnace, and the temperature is increased to 500° C. at a rate of 5° C. / min and calcined for 2 h to obtain a nitrogen-doped copper oxide / carbon composite material.
[0058] That is, Comparative Example 2 is substantially the same as Example 1, except that it does not contain manganese sulfate monohydrate.
[0059] Comparative Example 3
[0060] This comparative example provides a method for preparing a nitrogen-doped carbon composite material, which specifically comprises the following steps:
[0061] S1. Pour 10 g of urea and 4 g of oxalic acid into a mortar and mix and grind for 10 min until the materials are evenly mixed to obtain a mixture;
[0062] S2. The mixture obtained in step S1 is transferred into a covered crucible, and then the crucible is placed in a muffle furnace, and the temperature is increased to 500° C. at a rate of 5° C. / min and calcined for 2 h to obtain a nitrogen-doped carbon composite material.
[0063] That is, Comparative Example 3 is substantially the same as Example 1, except that it does not contain manganese sulfate monohydrate and copper sulfate pentahydrate.
[0064] Experimental example
[0065] Five 50 mL portions of 50 mg / L BPA solution were prepared, and 25 mg of the composite materials prepared in Example 1 and Comparative Examples 1 to 3 were added in sequence as catalysts. The remaining portion without the composite material was used as a blank control group, and magnetic stirring was performed in the dark for 10 min to reach adsorption-desorption equilibrium; then 0.4 mL of PMS (0.4 g / L) solution was quickly added to carry out degradation reaction, and the reaction was started. Samples were taken for testing after 0 min, 0.5 min, 1 min, 2 min, 3 min, 5 min, 7 min and 9 min, respectively.
[0066] Figure 4 The efficiency diagram of the composite material prepared in Example 1 and Comparative Examples 1 to 3 in activating PMS to degrade BPA; Figure 4 It can be seen that, compared with single PMS, nitrogen-doped carbon material, nitrogen-doped copper oxide / carbon composite material and nitrogen-doped manganese tetraoxide / carbon composite material, the nitrogen-doped copper manganate / carbon composite material prepared by the present invention has an excellent catalytic effect on PMS, can efficiently activate PMS to quickly degrade BPA, and can completely degrade BPA within 9 minutes; This shows that the composite material of the present invention can activate PMS to quickly and completely degrade BPA in a short time, greatly improving the efficiency of PMS in degrading BPA.
[0067] Figure 5 This is a diagram of the BPA mineralization effect of the composite material prepared in Example 1. Figure 5 It can be seen that the TOC removal rate reaches more than 98% within 9 minutes, with a very high mineralization rate, and the TOC removal rate is basically synchronized with the degradation rate of BPA, indicating that the composite material of the present invention can catalyze PMS to completely degrade BPA into CO2 and H2O without producing other intermediates.
[0068] Figure 6 The BPA degradation efficiency diagram under different manganese-copper ratios is shown in Figure 2. Figure 6 It can be seen that when the molar ratio of manganese salt to copper salt is 2:1, the nitrogen-doped copper manganate / carbon composite material has the best catalytic effect on PMS.
[0069] Figure 7 The degradation efficiency diagram of the composite material of Example 1 after 4 times of degradation of BPA solution is shown in FIG. Figure 7 It can be seen that the composite material prepared by the present invention can be reused without obvious attenuation of catalytic activity, and the degradation rate of BPA can still reach more than 85% when used for the fourth time, indicating that the composite material prepared by the preparation method of the present invention has good recyclability as a catalyst.
[0070] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a nitrogen-doped copper manganate / carbon composite material, characterized in that: The following steps are involved: S1. The urea, organic acid, manganese salt and copper salt are mixed and ground to obtain a mixture; S2. calcining the mixture obtained in step S1 at 500-600° C. for 1-4 h to obtain the nitrogen-doped copper manganate / carbon composite material; In step S1, the organic acid includes at least one of oxalic acid, citric acid, and tartaric acid; the molar ratio of the manganese salt to the copper salt is (1-5):1; and the mass molar ratio of the total amount of urea, organic acid, manganese salt and copper salt is (0.5-10) g:(1-4) g:0.6 mmol.
2. The method for preparing a nitrogen-doped copper manganate / carbon composite material according to claim 1, characterized in that: In step S1, the manganese salt includes one of manganese sulfate, manganese chloride and manganese nitrate, and the copper salt includes one of copper sulfate, copper chloride and copper nitrate.
3. The method for preparing a nitrogen-doped copper manganate / carbon composite material according to claim 1, characterized in that: In step S2, the calcination temperature is 500°C and the time is 2 hours.
4. The method for preparing a nitrogen-doped copper manganate / carbon composite material according to claim 1, characterized in that: In step S1, the molar ratio of the manganese salt to the copper salt is 2:
1.
5. A nitrogen-doped copper manganate / carbon composite material activated with persulfate, characterized in that: The method is prepared according to any one of claims 1 to 4.
6. Use of the nitrogen-doped copper manganate / carbon composite material of activated persulfate according to claim 5 in degrading organic pollutants, characterized in that: The method is as follows: adding the nitrogen-doped copper manganate / carbon composite material of activated persulfate into organic pollutants, placing it in a dark place to reach adsorption equilibrium, and then adding a persulfate solution to carry out degradation reaction.
7. The use according to claim 6, characterized in that: The organic pollutant is BPA, and the persulfate is peroxymonosulfate or peroxydisulfate.
Citation Information
Patent Citations
Renewable cyclic utilization mercury adsorbent as well as preparation method and regeneration method thereof
CN107601570A
Method for degrading bisphenol A in water based on manganese oxide modified copper-manganese spinel
CN113772802A