Formation method of high-capacity liquid metal battery

By using a method of gradually increasing the discharge rate after low-magnification deep charging and discharging in large-capacity liquid metal batteries, the optimization process is solved, the problem of long battery activation cycle is achieved, and the efficient and rapid transformation process is achieved, and the efficiency and transformation of Coulomb are improved. quality.

CN119050517AActive Publication Date: 2024-11-29WUHAN JIZHAO ENERGY STORAGE TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411167360.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

During the initial charging and discharging process of large-capacity liquid metal batteries, there are problems such as low mass transfer efficiency, uneven current density distribution, unstable electrode/electrolyte interface and low utilization rate of active materials, resulting in long activation cycles and low efficiency, making it difficult to meet industrial production. demand.

Method used

A method of synthesis is adopted to carry out deep charging and discharge from low magnifications, initially build a stable electrode/electrolyte interface, and gradually increase the discharge rate, optimize the discharge depth and cycle number, combine to increase the activation temperature, shorten the transformation time, and improve the transformation efficiency. .

Benefits of technology

The battery synthesis time has been shortened to 2 days, and the Coulomb efficiency has been maintained at more than 98%, reducing the production cost, avoiding battery short-circuit failure, and improving activation quality and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050517A_ABST
    Figure CN119050517A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of liquid metal batteries, in particular to a formation method of a high-capacity liquid metal battery. According to the formation method of the high-capacity liquid metal battery, deep charging and discharging are carried out from the first circle at a low rate, a relatively stable electrode / electrolyte interface is preliminarily constructed, meanwhile, a positive electrode active material is utilized to the greatest extent, then, the discharging rate is properly improved, shallow charging and shallow discharging are carried out at the same discharging depth, and thus the formation of the high-capacity liquid metal battery is realized. And gradually consolidating the stable electrode / electrolyte interface and activating the positive electrode active material at the same time, so that the positive electrode active material is fully utilized, and finally battery formation is completed. Besides, an optimization method combining a series of means of improving the discharge rate, reducing the discharge depth, reducing the number of cycles, improving the activation temperature and the like is provided for factors influencing the formation duration and quality of the high-capacity liquid metal battery, boundary conditions of high-quality formation of the high-capacity liquid metal battery are explored, the formation duration of the battery is shortened as much as possible, and the formation efficiency of the battery is improved. The formation efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of liquid metal batteries, and in particular to a formation method of a large-capacity liquid metal battery. Background Art

[0002] At present, the research on liquid metal batteries is becoming more and more mature and is about to enter the industrialization stage. Similar to most battery systems, batteries need to have an activation process, that is, a formation process, before use. Only after the formation of the battery can it maintain a stable state of high coulombic efficiency and full capacity charge and discharge when it is officially used. The difference is that due to the large capacity of liquid metal battery cells (200-500Ah), thick electrode and electrolyte materials, and large reaction interface area, the battery will have low mass transfer efficiency, uneven current density distribution, unstable electrode / electrolyte interface, and low utilization of active materials during the initial charge and discharge process. Therefore, the battery requires a longer activation process to build a stable electrode / electrolyte interface and achieve stable and efficient mass transfer and utilization of active substances. In the battery activation stage, the high-rate charge and discharge mode will aggravate the uneven distribution of current density inside the battery, and it is very easy to produce rapid enrichment of melt in areas with high current density, causing battery short circuit. Therefore, the formation process commonly used in large-capacity battery cells at present is to gradually build a stable electrode / electrolyte interface under low rate (generally 0.05-0.1C) from shallow (20-30%) to deep constant current charge and discharge (60-80% DOD) mode (see CN106981691B for details, a large-capacity liquid metal battery interface formation method). Although this progressive formation step can achieve the activation of large-capacity batteries, the battery activation cycle is too long, generally 1-2 weeks, and the activation efficiency is low. For industrial production, the production cost is high and the production efficiency is low. Therefore, it is urgent to develop a fast and efficient formation method for large-capacity liquid metal batteries to achieve cost reduction and efficiency improvement. Summary of the invention

[0003] The purpose of the present invention is to provide a formation method for a large-capacity liquid metal battery in view of the above-mentioned deficiencies in the prior art.

[0004] A formation method of a large-capacity liquid metal battery of the present invention comprises the following steps:

[0005] S1. Place the large-capacity liquid metal battery in the test furnace and connect the test instrument to heat it to the working temperature;

[0006] S2. After the large-capacity liquid metal battery is heated to the operating temperature, the test program is started to detect the voltage change of the large-capacity liquid metal battery. After the voltage of the large-capacity liquid metal battery is normal and the fluctuation is small, it is put on hold for a predetermined time;

[0007] S3, discharging the large-capacity liquid metal battery at a small rate constant current to a cut-off voltage, so that the discharge depth of the large-capacity liquid metal battery is 80% DOD to 100% DOD;

[0008] S4, after the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is charged at a small rate or a medium rate constant current to a cut-off voltage;

[0009] After the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is discharged at a small rate or a medium rate constant current, and the discharge time is controlled so that the discharge depth of the large-capacity liquid metal battery is 20% DOD to 80% DOD;

[0010] Wherein, after step S4 is performed 0-6 times, if the coulombic efficiency of the large-capacity liquid metal battery is less than 95%, the following steps S5 to S7 are continued; if the coulombic efficiency of the large-capacity liquid metal battery is greater than or equal to 95%, the battery activation is completed, and the following steps S5 to S7 do not need to be performed;

[0011] S5, after the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is charged at a small rate or a medium rate constant current to a cut-off voltage;

[0012] After the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is discharged at a small rate or a medium rate constant current to a cut-off voltage, so that the discharge depth of the large-capacity liquid metal battery is 80% DOD to 100% DOD;

[0013] S6, after the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is charged at a small rate or a medium rate constant current to a cut-off voltage;

[0014] After the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is discharged at a small rate or a medium rate constant current, and the discharge time is controlled so that the discharge depth of the large-capacity liquid metal battery is 20% DOD to 80% DOD;

[0015] S7, repeat step S6 until the coulombic efficiency of the large-capacity liquid metal battery is greater than or equal to 95%, and the battery activation is completed.

[0016] Furthermore, when the large-capacity liquid metal battery is charged and discharged, the small rate is 0.05-0.15C, and the medium rate is 0.15-0.5C.

[0017] Furthermore, when the large-capacity liquid metal battery is charged and discharged, the small rate is 0.1C and the medium rate is 0.2C.

[0018] Furthermore, the predetermined time of step S2 is 2 hours.

[0019] Further, step S4 is performed twice before step S5 is performed.

[0020] Further, in step S7, step S6 is repeated 0 to 6 times.

[0021] Furthermore, in step S4, the depth of discharge is 40% DOD to 75% DOD.

[0022] Furthermore, the total formation time does not exceed 80 hours.

[0023] The present invention is contrary to the design concept of the current progressive formation method of large-capacity liquid metal batteries. The formation method of the large-capacity liquid metal battery of the present invention performs deep charge and discharge at a low rate from the first cycle, initially constructs a relatively stable electrode / electrolyte interface, and maximizes the use of positive electrode active materials. Subsequently, the discharge rate is appropriately increased, and shallow charge and discharge are performed at the same discharge depth, gradually consolidating the stable electrode / electrolyte interface while activating the positive electrode active materials, so that the positive electrode active materials are fully utilized, and finally the battery formation is completed. In addition, for the factors that affect the formation time and quality of large-capacity liquid metal batteries, an optimization method combining a series of means such as increasing the discharge rate, reducing the discharge depth, reducing the number of cycles, and increasing the activation temperature is proposed to explore the boundary conditions for high-quality formation of large-capacity liquid metal batteries, shorten the battery formation time as much as possible, and improve the formation efficiency.

[0024] The formation method of a large-capacity liquid metal battery provided by the present invention mainly has the following beneficial effects:

[0025] (1) The performance of the large-capacity liquid metal battery formed by the method of the present invention is excellent. After the formation is completed, the battery is fully charged and discharged at a rate of 0.2C. The coulomb efficiency of each cycle of the battery is maintained above 98%. The optimal coulomb efficiency can be maintained above 99% for stable operation, and the formation quality is high and efficient;

[0026] (2) The method of the present invention is used to form a large-capacity liquid metal battery, and the formation time is shortened to within 2 days (46 hours). Compared with the currently common large-capacity liquid metal battery formation method, the formation time is shortened by at least 62 to 86%, greatly improving the formation efficiency and reducing the formation cost.

[0027] (3) Using a low-rate, deep charge-discharge mode during the first cycle of battery operation can initially build a relatively stable electrode / electrolyte interface and activate the positive electrode active material to participate in the electrochemical reaction to the greatest extent, thereby improving the activation quality and effectively avoiding battery short-circuit failure;

[0028] (4) During the first cycle of charge and discharge, the battery reaction interface has been initially formed. At this time, the battery enters a shallow charge and discharge mode, which can not only consolidate the formed electrode / electrolyte interface, but also gradually activate a small amount of remaining positive electrode active materials, while reducing the activation time.

[0029] (5) An optimization method combining a series of measures such as increasing the discharge rate, reducing the discharge depth, reducing the number of cycles, and increasing the activation temperature was proposed to achieve efficient activation of large-capacity liquid metal batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a flow chart of the formation method of the large-capacity liquid metal battery provided by the present invention;

[0031] Figure 2 , 3 , 4, and 5 are flow charts of the formation methods of large-capacity liquid metal batteries corresponding to Examples 1, 2, 3, and 4, respectively;

[0032] Figure 6 It is a comparison chart of the benefits obtained by the formation method of a large-capacity liquid metal battery of the present invention and the benefits obtained by the formation method of a large-capacity liquid metal battery provided by Chinese patent CN106981691B. DETAILED DESCRIPTION

[0033] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0034] Figure 1 The present invention is a flow chart of a formation method for a large-capacity liquid metal battery.

[0035] Table 1 lists four embodiments of the present invention, each of which includes 2 to 4 specific implementation cases of 200Ah batteries.

[0036] Example 1

[0037] like Figure 2 As shown, this embodiment uses a liquid metal battery with a capacity of 200Ah (referred to as batteries 1, 2, 3, and 4), and the formation method mainly includes the following steps:

[0038] (1) Batteries No. 1, 2, 3, and 4 are placed in four heating furnaces respectively, and the temperatures of the batteries No. 1, 2, 3, and 4 are raised to the working temperature at a heating rate of 4° C. / min.

[0039] (2) When the temperature of batteries 1, 2, 3, and 4 reaches the operating temperature, start the battery test program and detect the voltage of batteries 1, 2, 3, and 4. After the voltage of batteries 1, 2, 3, and 4 stabilizes, leave it alone for 2 hours.

[0040] (3) Perform constant current discharge on batteries 1, 2, 3, and 4 with a discharge rate of 0.1C (20A). At the same time, control the discharge cut-off voltage so that the discharge depth of batteries 1, 2, 3, and 4 is 100% DOD.

[0041] (4) After leaving batteries No. 1, 2, 3, and 4 for 10 minutes, charge them with constant current until they are fully charged, with a charging rate of 0.1C (20A).

[0042] (5) After leaving batteries No. 1, 2, 3, and 4 for 10 minutes, they are discharged at a constant current with a discharge rate of 0.1C (20A). At the same time, the discharge time is controlled to be 450 minutes (7.5 hours), so that the discharge depth of batteries No. 1, 2, 3, and 4 is 75% DOD.

[0043] (6) After leaving batteries No. 1, 2, 3, and 4 for 10 minutes, they are charged with constant current to the cut-off voltage at a charging rate of 0.1C (20A).

[0044] (7) Go to step (5) and repeat this cycle for 4 times.

[0045] (8) Batteries 1, 2, 3, and 4 are discharged at a constant current with a discharge rate of 0.2C (40A). At the same time, the discharge cut-off voltage is controlled so that the discharge depth of batteries 1, 2, 3, and 4 is 100% DOD.

[0046] (9) After leaving batteries No. 1, 2, 3, and 4 for 10 minutes, they are charged with constant current to the cut-off voltage at a charging rate of 0.2C (40A).

[0047] (10) After leaving batteries No. 1, 2, 3, and 4 for 10 minutes, they are discharged at a constant current with a discharge rate of 0.2C (40A) and a discharge time of 225 minutes (3.75 hours) to achieve a discharge depth of 75% DOD for batteries No. 1, 2, 3, and 4.

[0048] (11) After leaving batteries No. 1, 2, 3, and 4 for 10 minutes, they are charged with constant current to the cut-off voltage at a charging rate of 0.2C (40A).

[0049] (12) Go to step (10) and repeat the cycle for 4 cycles until the coulombic efficiency of batteries 1, 2, 3, and 4 is greater than or equal to 95%, and the battery formation is completed.

[0050] The formation time is 79 hours.

[0051] Verify the formation quality and stability of the formation battery:

[0052] (13) After leaving batteries No. 1, 2, 3, and 4 for 10 minutes, they are discharged at a constant current with a discharge rate of 0.2C (40A). At the same time, the discharge cut-off voltage is controlled so that the discharge depth of batteries No. 1, 2, 3, and 4 is 100% DOD.

[0053] (14) After leaving batteries No. 1, 2, 3, and 4 for 10 minutes, they are charged with constant current to the cut-off voltage at a charging rate of 0.2C (40A).

[0054] (15) Go to step (13) and repeat the cycle for 3 cycles. Record the discharge capacity and coulomb efficiency of the battery in each cycle as a verification standard for whether the formation battery is qualified.

[0055] Table 2 shows the specific parameters of No. 1, 2, 3, and 4 batteries after they were formed. The batteries were charged and discharged for 3 cycles at 0.2C (40A). This further verifies the formation quality and stability of the formed batteries.

[0056] Example 2

[0057] like Figure 3 As shown, this embodiment uses a liquid metal battery with a capacity of 200Ah (referred to as No. 5 and No. 6 batteries). The main steps of the formation method are similar to those of Example 1, except that the discharge depth is reduced and the number of cycles is reduced in steps (5)-(7), and the discharge depth is reduced in steps (10)-(12). The specific parameters are shown in Example 2 in Table 1.

[0058] The formation time is 60 hours.

[0059] Table 3 shows the specific parameters of No. 5 and No. 6 batteries after they were formed. The batteries were charged and discharged for 3 cycles at 0.2C (40A). This further verifies the formation quality and stability of the formed batteries.

[0060] Example 3

[0061] like Figure 4 As shown, this embodiment uses a liquid metal battery with a capacity of 200Ah (denoted as batteries 7, 8, 9, and 10). The main steps of the formation method are similar to those of Example 1, except that there are no steps (5)-(7), and in steps (10)-(12), the discharge depth is reduced. The specific parameters are shown in Example 3 in Table 1.

[0062] The formation time is 50 hours.

[0063] Table 4 shows the specific parameters of No. 7, 8, 9, and 10 batteries after they were formed. The batteries were charged and discharged for 3 cycles at 0.2C (40A). This further verifies the formation quality and stability of the formed batteries.

[0064] Example 4

[0065] like Figure 5 As shown, this embodiment uses a liquid metal battery with a capacity of 200Ah (denoted as batteries 7, 8, 9, and 10). The main steps of the formation method are similar to those of Example 1, except that there are no steps (5)-(7), and in steps (10)-(12), the discharge depth is reduced. The specific parameters are shown in Example 3 in Table 1.

[0066] The formation time is 46 hours.

[0067] Table 5 shows the specific parameters of No. 11, 12, 13, and 14 batteries after they were formed. The batteries were charged and discharged for 3 cycles at 0.2C (40A). This further verifies the formation quality and stability of the formed batteries.

[0068] Table 1

[0069]

[0070] Table 2 Table 3 Table 4

[0071]

[0072] Table 5

[0073]

[0074] It can be seen from Tables 2-5 that the coulombic efficiency of the batteries obtained by the formation method of the present invention is above 98%.

[0075] Figure 6 This is a comparison chart of the benefits obtained by the formation method of the large-capacity liquid metal battery of the present invention and the benefits obtained by the formation method of the large-capacity liquid metal battery provided by Chinese patent CN106981691B. It can be seen from the figure that the formation method of the present invention takes less formation time and the coulombic efficiency of the obtained battery is high.

[0076] For matters not mentioned above, the prior art applies.

[0077] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A formation method for a large-capacity liquid metal battery, characterized in that: The following steps are involved: S1. Place the large-capacity liquid metal battery in the test furnace and connect the test instrument to heat it to the working temperature; S2. After the large-capacity liquid metal battery is heated to the operating temperature, the test program is started to detect the voltage change of the large-capacity liquid metal battery. After the voltage of the large-capacity liquid metal battery is normal and the fluctuation is small, it is put on hold for a predetermined time; S3, discharging the large-capacity liquid metal battery at a small rate constant current to a cut-off voltage, so that the discharge depth of the large-capacity liquid metal battery is 80% DOD to 100% DOD; S4, after the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is charged at a small rate or a medium rate constant current to a cut-off voltage; After the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is discharged at a small rate or a medium rate constant current, and the discharge time is controlled so that the discharge depth of the large-capacity liquid metal battery is 20% DOD to 80% DOD; Wherein, after step S4 is performed 0-6 times, if the coulombic efficiency of the large-capacity liquid metal battery is less than 95%, the following steps S5 to S7 are continued; if the coulombic efficiency of the large-capacity liquid metal battery is greater than or equal to 95%, the battery activation is completed, and the following steps S5 to S7 do not need to be performed; S5, after the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is charged at a small rate or a medium rate constant current to a cut-off voltage; After the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is discharged at a small rate or a medium rate constant current to a cut-off voltage, so that the discharge depth of the large-capacity liquid metal battery is 80% DOD to 100% DOD; S6, after the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is charged at a small rate or a medium rate constant current to a cut-off voltage; After the large-capacity liquid metal battery is left for 5 to 30 minutes, the large-capacity liquid metal battery is discharged at a small rate or a medium rate constant current, and the discharge time is controlled so that the discharge depth of the large-capacity liquid metal battery is 20% DOD to 80% DOD; S7, repeat step S6 until the coulombic efficiency of the large-capacity liquid metal battery is greater than or equal to 95%, and the battery activation is completed.

2. A formation method for a large-capacity liquid metal battery as claimed in claim 1, characterized in that: When the large-capacity liquid metal battery is charged and discharged, the small rate is 0.05-0.15C, and the medium rate is 0.15-0.5C.

3. A formation method for a large-capacity liquid metal battery as claimed in claim 2, characterized in that: When the large-capacity liquid metal battery is charged and discharged, the small rate is 0.1C and the medium rate is 0.2C.

4. The formation method of a large-capacity liquid metal battery according to claim 1, characterized in that: The scheduled time for step S2 is 2 hours.

5. The formation method of a large-capacity liquid metal battery according to claim 1, characterized in that: Step S4 is performed twice before performing step S5.

6. A formation method for a large-capacity liquid metal battery as claimed in claim 1, characterized in that: In step S7, step S6 is repeated 0 to 6 times.

7. A formation method for a large-capacity liquid metal battery as claimed in claim 1, characterized in that: In step S4, the depth of discharge is 40% DOD to 75% DOD.

8. The formation method of a large-capacity liquid metal battery according to claim 1, characterized in that: The total formation time shall not exceed 80h.

Citation Information

Patent Citations

  • A method for interfacial formation of high-capacity liquid metal batteries

    CN106981691B

  • Lithium secondary cell with high charge and discharge rate capability and low impedance growth

    CN102544496A

  • Interface formation method of large-capacity liquid metal battery

    CN106981691A

  • Restore method of liquid-state metal battery

    CN107732335A

  • Cu < + > / Li < + > dual-ion conductor and high-power all-solid-state lithium battery

    CN117317352A