A kind of high-toughness hot-rolled steel strip with thick gauge and yield strength of 600MPa and its production method

By using low carbon, medium manganese, titanium-niobium composite micro-alloying and an appropriate amount of chromium composition design in thick-gauge hot-rolled strips, combined with clean steel smelting-continuous casting and controlled rolling and controlled cooling processes, the problem of thick-gauge hot-rolled strips can be solved Addressing the issue of low-temperature impact toughness of strip steel in low-temperature environments, we have achieved the production of high-toughness and low-cost 600MPa grade hot-rolled strip steel, which is suitable for the use of engineering machinery in low-temperature environments.

CN116445818BActive Publication Date: 2024-10-11SD STEEL RIZHAO CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202310416744.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-11
Estimated Expiration
2043-04-13

AI Technical Summary

Technical Problem

In the existing technology, hot-rolled strip steel with a yield strength greater than 600MPa and a thickness of 12 mm or more has unstable low-temperature impact toughness and poor impact value in a low-temperature environment, making it difficult to meet the requirements for use in low-temperature environments.

Method used

It adopts the composition design of low carbon, medium manganese, titanium-niobium composite micro-alloying and appropriate amount of chromium, and combines the clean steel smelting-continuous casting process and controlled rolling and controlled cooling process to control the chemical composition and production process parameters of the steel billet to produce high toughness The 600MPa thick hot-rolled strip steel has excellent low-temperature toughness and is suitable for engineering machinery and equipment serving in low-temperature environments.

Benefits of technology

It achieves the stable production of 600MPa hot-rolled strip steel with thick specifications, high strength and high toughness, which meets the usage conditions of steel for various engineering machinery. It is especially suitable for engineering machinery and equipment serving in low-temperature environments. The amount of alloy added is small. The material cost is low and the process is simple and easy to implement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116445818B_ABST
    Figure CN116445818B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of metallurgy, and in particular to a high-toughness hot-rolled strip steel with a yield strength of 600 MPa and a production method thereof. The chemical components and mass percentages thereof are respectively C: 0.07%-0.10%, Si: 0.15%-0.30%, Mn: 1.60%-1.75%, P≤0.018%, S≤0.0040%, Ti: 0.055%-0.070%, Nb: 0.050%-0.065%, Cr: 0.10%-0.20%, Al: 0.020%-0.050%, N≤0.0040%, and the rest are Fe and unavoidable impurities. The present invention adopts low carbon, medium manganese, titanium-niobium composite microalloying and appropriate chromium composition design and appropriate component ratio, combines clean steel smelting-continuous casting process and appropriate controlled rolling and controlled cooling process, and produces thick-gauge 600MPa grade hot-rolled strip steel with excellent low-temperature toughness and stable comprehensive performance. It is suitable for use in engineering machinery equipment serving in low-temperature environments, has a small amount of precious alloy addition, low material cost, simple and easy process, and is easy to industrialize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to a thick-gauge high-toughness hot-rolled strip steel with a yield strength of 600 MPa and a production method thereof. Background Art

[0002] In the construction machinery industry, low alloy high strength steel is widely used due to its low material cost and high mechanical properties. With the development of modern industry, construction machinery is gradually developing towards large-scale equipment, lightweight and complex service environment, and the comprehensive performance requirements for steel used in construction machinery are also getting higher and higher. Among them, due to the expansion of the service environment, some construction machinery needs to operate for a long time in a low temperature environment, requiring steel to have not only high strength, good forming and welding properties, but also excellent impact toughness, especially low temperature impact toughness. Otherwise, cracking problems are likely to occur during use, leading to equipment and production accidents, and even causing personal injury.

[0003] In the prior art, engineering machinery steel with a thickness of 12-16mm mainly uses cost-effective hot-rolled strip Kaiping products. Among them, titanium-reinforced hot-rolled strip steel that applies the principle of titanium microalloying is favored in the development of high-strength hot-rolled strip steel due to its significant strengthening effect and ultra-low alloy addition cost. It is often used to produce 600MPa-level high-strength thick-gauge hot-rolled strip steel.

[0004] However, as the strength level and thickness increase, the toughness of hot-rolled strip generally shows a downward trend, and the decline in toughness of hot-rolled strip reinforced with titanium is particularly obvious. When producing hot-rolled strip with a yield strength greater than 600MPa and a thickness of 12mm or more, the problem of poor and unstable low-temperature impact toughness of titanium-reinforced hot-rolled strip is extremely prominent, making it difficult to meet the requirements for use in low-temperature environments.

[0005] Patent CN104831167 B discloses a Q550E high-strength steel hot-rolled coil and its production method, which adopts a Nb-V-Ti composite microalloying component system, with high final rolling temperature and coiling temperature. The specific thickness is not provided and the actual low-temperature toughness index is not described.

[0006] Patent CN112828036B discloses a method for improving the low-temperature impact toughness of thick-gauge high-strength steel. It requires that the steel temperature before the finishing mill be ≥509 to ensure that the rough rolling end temperature is ≤1040℃. It has strict restrictions on dephosphorization water, inter-frame cooling water, strip speed, etc., resulting in low production efficiency and great difficulty in process control.

[0007] Patent CN110306124A discloses a low-cost Ti microalloyed 620MPa grade hot-rolled strip and production method, which adopts a low-cost component design of medium carbon (0.15-0.18%) and titanium microalloyed (0.08-0.12%), and produces 1-3mm thin gauge 620MPa grade hot-rolled strip.

[0008] In summary, there is an urgent need to develop 600MPa grade 12-16mm thick hot-rolled strip steel with economical cost, simple process and excellent low-temperature toughness, so as to better meet the market demand for thick-gauge, high-strength and tough engineering machinery steel. Summary of the invention

[0009] In view of the technical problems in the prior art that the low-temperature impact toughness of hot-rolled steel strips with a yield strength greater than 600 MPa and a thickness of more than 12 mm is unstable and the impact value is poor, making it difficult to meet the requirements for use in a low-temperature environment, the present invention provides a high-toughness hot-rolled steel strip with a yield strength of 600 MPa and a thick specification, and a production method thereof. The high-toughness hot-rolled steel strips are produced by adopting a low-carbon, medium-manganese, titanium-niobium composite microalloying and a composition design of an appropriate amount of chromium and a suitable composition ratio, combined with a clean steel smelting-continuous casting process and a controlled rolling and controlled cooling process. The high-toughness thick-specification 600 MPa hot-rolled steel strips have excellent low-temperature toughness and stable comprehensive performance, are suitable for use in engineering machinery equipment serving in a low-temperature environment, have a small amount of precious alloy addition, have a low material cost, are simple and easy to process, and are easy to industrialize.

[0010] In the first aspect, the present invention provides a method for producing thick-gauge high-toughness hot-rolled strip steel with a yield strength of 600 MPa, comprising smelting, continuous casting, heating, rolling, cooling and coiling processes, wherein the chemical composition and mass percentage of the steel billet are respectively C: 0.07%-0.10%, Si: 0.15%-0.30%, Mn: 1.60%-1.75%, P≤0.018%, S≤0.0040%, Ti: 0.055%-0.070%, Nb: 0.050%-0.065%, Cr: 0.10%-0.20%, Al: 0.020%-0.050%, N≤0.0040%, and the rest are Fe and unavoidable impurities.

[0011] Chemical composition has an important influence on product performance. The present invention imposes restrictions on the chemical composition of the steel billet, as described below.

[0012] C: Carbon is the main solid solution strengthening element in steel, which can significantly improve the strength of steel, but too high a carbon content is detrimental to the toughness and welding performance of steel. At the same time, in order to give full play to the precipitation strengthening and fine grain strengthening effects of Ti and Nb microalloying elements, the present invention limits the carbon content to 0.07%-0.10%.

[0013] Si: Silicon is also an important solid solution strengthening element and has a deoxidizing effect, but too high a silicon content will affect the surface quality, welding performance and low-temperature toughness of the steel. The silicon content of the present invention is controlled at 0.15%-0.30%.

[0014] Mn: Manganese is an important strengthening and toughening alloy element with a strong solid solution strengthening effect. It can reduce the phase transition temperature of steel and refine the structure of steel. However, Mn is also an element that is easy to segregate. When the content is too high, it will have an adverse effect on the toughness of steel and increase the sensitivity of welding cracks. The manganese content of the present invention is controlled at 1.60%-1.75%.

[0015] P: Phosphorus increases the cold brittleness of steel and deteriorates welding performance. It is a harmful element and its content should be reduced as much as possible. In the present invention, the phosphorus content is controlled to be ≤0.018%.

[0016] S: Sulfur is also a harmful element, which has a great impact on the toughness and plasticity of steel. When the content is too high, it is easy to form micron-sized precipitation phases with titanium at high temperature, which deteriorates the toughness of steel. The sulfur content in steel should be strictly controlled. In the present invention, the sulfur content is controlled at ≤0.004%.

[0017] Ti: As a microalloying element, titanium can play a significant precipitation strengthening role and a certain degree of fine grain strengthening role in steel in combination with appropriate production processes, significantly improving the strength of steel. At the same time, due to its low cost, it can replace some precious alloy elements and significantly reduce the alloy cost. However, the Ti content should not be too high, otherwise it is easy to form large-sized titanium-containing precipitation phases, which will deteriorate the low-temperature toughness of steel, especially thick-gauge products. At the same time, its role is significantly affected by the content of elements such as carbon, niobium, and nitrogen. The titanium content of the present invention is controlled at 0.055%-0.070%.

[0018] Nb: Niobium is a microalloying element that can increase the recrystallization temperature of austenite and expand the rolling range of the non-recrystallization zone. Its carbonitride precipitates at defects such as dislocations and grain boundaries, which can inhibit austenite recrystallization and prevent grain growth, and provide energy and position for ferrite nucleation, significantly refine grains, and improve the strength and toughness of steel. However, its role is affected by the content of elements such as carbon and titanium. At the same time, considering its cost, the niobium content in the present invention is controlled at 0.050%-0.065%.

[0019] Cr: Chromium can improve the hardenability of steel, and the effect is stronger when used in combination with manganese. It can improve the uniformity of the steel structure and the stability of its performance in the thickness direction. However, too high a chromium content will increase the sensitivity of welding cracks and affect the weldability of the steel. Therefore, the chromium content in the present invention is controlled at 0.10%-0.20%.

[0020] Al: Aluminum can effectively deoxidize during the steelmaking process and also play a role in refining the structure, but the content should not be too high, otherwise it is easy to cause cracks in the casting. Therefore, the aluminum content in the present invention is controlled to be 0.020%-0.050%.

[0021] Furthermore, the smelting process adopts LF+RH double refining process to ensure the purity of molten steel; titanium-iron alloy is added to the RH furnace. Since the RH furnace can perform vacuum degassing, the oxygen content is greatly reduced, which can avoid oxidation of titanium; the vacuum holding time is ≥12min, the pure degassing time is ≥7min, and the soft blowing time is ≥12min.

[0022] Furthermore, argon is used to protect the pouring throughout the continuous casting process to prevent secondary oxidation of the molten steel; low superheat and constant pulling speed control are adopted, with the superheat being 15-25°C and the billet pulling speed being 1.0-1.2m / min, to ensure stable billet quality.

[0023] Furthermore, the ALoW intercooling mode is used for cooling in the continuous casting process, the secondary cooling water volume ratio is 0.80-0.90 L / kg, and the cooling rate is controlled at 7-9°C / s. The higher cooling rate avoids the generation of micron-sized TiN precipitation phase that is detrimental to toughness at high temperatures; the continuous casting billet thickness is 230 mm.

[0024] Furthermore, in the heating process, the temperature of the soaking section is 1220-1260°C, the soaking time is 30-60min, and the temperature out of the heating furnace is 1200-1240°C; the total heating time in the furnace is 180-260min, so that the ingot is completely austenitized and the titanium-containing precipitate phase is fully dissolved, while avoiding the coarsening of the austenite grains.

[0025] Furthermore, the rolling process is divided into rough rolling and finishing rolling. Based on the influence of the content of elements such as niobium and carbon on the austenite recrystallization temperature under the conditions of this patent, the austenite recrystallization temperature is above 1032°C, and the rough rolling final rolling temperature (R2DT) is 1040-1080°C, which can ensure that the rough rolling is completely carried out in the recrystallization zone. The intermediate billet is obtained by 5 round-trip rolling. The grains are refined by repeated recrystallization of austenite during the round-trip rolling process; the thickness of the intermediate billet is 46-56mm, which ensures that the total reduction rate of the rough rolling process is above 75%, avoids incomplete recrystallization of austenite due to insufficient rough rolling compression ratio, and then produces mixed crystal phenomenon, reduces the uniformity of the steel structure, and affects the low-temperature toughness of the steel; at the same time, the thickness of the intermediate billet should be at least 3.5 times the thickness of the finished steel strip, so as to ensure sufficient deformation during the finishing rolling process. The austenite grains are fully flattened and crushed in the non-recrystallized area during rolling, the austenite grains are refined, and the uniformity of the organization is improved; the finishing entry temperature (FET) is 1000-1030°C, which can ensure that the finishing rolling is carried out in the non-recrystallized area; the finishing rolling adopts 7-pass continuous rolling of the stand, the finishing final rolling temperature (FDT) is 840-870°C, and the reduction rate of the last pass in the finishing stage is ≥14%. Through this process, the austenite grains are fully refined to obtain the target organization grain size, and a large number of deformation structures such as dislocations and subgrain boundaries are obtained, which creates conditions for the subsequent final ferrite organization refinement and the precipitation of fine titanium-containing phases in the ferrite. If the finishing final rolling temperature is too low, the titanium-containing phase will be precipitated in austenite in a larger size in advance, reducing the strength and toughness of the final product; the strip thickness after finishing rolling is 12-16mm.

[0026] Furthermore, the cooling process adopts two-stage cooling, combined with the production line equipment configuration. In the first stage, on the basis of ensuring the stability of the plate shape, the steel is quickly cooled to a certain temperature, the cooling rate is 30-45℃ / s, the cooling outlet temperature (MT1) is 660-700℃, and the water pressure is controlled at 0.38-0.42MPa; the rapid cooling in the first stage can inhibit the pearlite phase transformation, promote the ferrite phase transformation, refine the ferrite grains, improve the cooling penetration ability, make the structure uniform in the thickness direction, and avoid the titanium-containing phase at high temperature. The cooling water precipitates during the phase change process. The water pressure range of this cooling water can improve the penetration capacity of water cooling in the production of thick-gauge strip steel, ensure that the strip steel is cooled in place at the thickness center and has a uniform structure, and avoid quality problems such as unstable production and deviation of the steel strip caused by excessive water pressure. The cooling rate in the second stage is 15-25℃ / s. Reducing the cooling rate at this stage can make the ferrite phase change more complete, promote the nucleation of fine TiC, (Ti,Nb)C and other carbides at the phase interface of austenite and ferrite, and play a precipitation strengthening role.

[0027] Furthermore, in the coiling process, the coiling temperature (CT) is 510-540℃, and the coiling is air-cooled to room temperature. This coiling process can avoid the formation of pearlite, refine the ferrite structure, and improve the strength and toughness of the steel. On the other hand, it can make a sufficient volume fraction and finer carbide precipitate in the supersaturated ferrite matrix, while ensuring the precipitation strengthening effect and reducing the adverse effect on toughness; the strip steel is thick and the temperature drops slowly, which provides the necessary time for the precipitation of carbides. After coiling, it can be directly cooled to room temperature in the air. If the coiling temperature is set too high, it will reduce the cooling rate in the cooling stage, which is easy to cause the formation of pearlite structure and the growth and coarsening of precipitated particles, which is not conducive to the toughness of the steel. If the coiling temperature is too low, it will not only increase the load of the coiler, leading to production difficulties, but also inhibit the precipitation of carbides, resulting in insufficient strength.

[0028] In a second aspect, the present invention provides a thick-gauge high-toughness hot-rolled steel strip with a yield strength of 600 MPa. The thickness of the steel strip is 12-16 mm, which belongs to a thick-gauge hot-rolled steel strip.

[0029] Furthermore, the steel strip has a yield strength of 600-700MPa, a tensile strength of 700-800MPa, an elongation of >20%, and an impact energy of >180J at -40°C, meeting the 600MPa-level strength standard and having strong low-temperature impact toughness.

[0030] The beneficial effects of the present invention are:

[0031] 1. The present invention fully cooperates with the steel composition and production process, adopts the composition design of low carbon, medium manganese, titanium-niobium composite microalloying and appropriate chromium and appropriate composition ratio, cooperates with appropriate production process design, especially controls the cooling water volume and cooling rate in the continuous casting process, controls the temperature and reduction rate of each link in the rolling process, and controls the parameters of the cooling and coiling links at the same time, so as to realize the stable production of thick-gauge, high-strength and high-toughness hot-rolled strip steel.

[0032] 2. The hot-rolled strip produced by the present invention has a thickness of 12-16 mm, a yield strength of 600-700 MPa, a tensile strength of 700-800 MPa, an elongation of >20%, and an impact energy of >180 J at -40°C. It is a high-toughness thick-specification 600 MPa grade hot-rolled strip steel, which can meet the use conditions of various engineering machinery steels and is particularly suitable for use in engineering machinery equipment serving in low temperature environments.

[0033] 3. The steel composition of the present invention has a small amount of alloy addition and a low raw material cost; at the same time, the operation and parameter control difficulty of each process in the production method is relatively low, the production process is simple and easy, and it is easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0035] Figure 1 This is the microstructure diagram of the hot-rolled strip in Example 1.

[0036] Figure 2 This is the microstructure diagram of the hot-rolled strip in Example 2.

[0037] Figure 3 This is the microstructure diagram of the hot-rolled strip in Example 3.

[0038] Figure 4 This is the microstructure diagram of the hot rolled strip in Comparative Example 3.

[0039] Figure 5 This is the microstructure diagram of the hot rolled strip in Comparative Example 4. DETAILED DESCRIPTION

[0040] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0041] Example 1

[0042] A high-toughness hot-rolled steel strip with a yield strength of 600 MPa. The thickness of the steel strip is 12.0 mm. The chemical composition and mass percentage of the steel billet are respectively C: 0.073%, Si: 0.25%, Mn: 1.64%, P: 0.014%, S: 0.0030%, Ti: 0.063%, Nb: 0.055%, Cr: 0.15%, Al: 0.033%, N: 0.0037%, and the rest are Fe and unavoidable impurities.

[0043] The production method includes smelting, continuous casting, heating, rolling, cooling and coiling processes. The key process controls are as follows:

[0044] (1) Smelting: LF+RH double refining is adopted, titanium-iron alloy is added to the RH furnace, the vacuum pressure holding time is 15 minutes, the pure degassing time is 8 minutes, and the soft blowing time is 13 minutes to obtain molten steel with good purity.

[0045] (2) Continuous casting: The whole process adopts argon protection pouring, low superheat control and constant pulling speed control, the superheat is 15℃, the billet pulling speed is 1.0m / min, the cooling uses the ALoW intercooling mode, the secondary cooling water volume is 0.83L / kg, the cooling rate is controlled at 7℃ / s, and the continuous casting billet thickness is 230mm.

[0046] (3) Heating: The temperature of the ingot heating and soaking section is 1232°C, the soaking time is 46 min, the ingot out-of-furnace temperature is 1223°C, and the heating time in the furnace is 214 min.

[0047] (4) Rolling: The final rolling temperature of the rough rolling is 1065°C, and the intermediate billet is obtained by rolling in 5 passes. The thickness of the intermediate billet is 46 mm. The final rolling temperature of the finishing rolling is 843°C, the rolling speed is 4 m / s, the reduction rate of the last pass in the finishing rolling stage is 16.4%, and the plate thickness after 7 passes of finishing rolling is 12.0 mm.

[0048] (5) Cooling: After rolling, two-stage cooling is adopted. In the first stage, the ultra-fast cooling outlet temperature is 686°C, the ultra-fast cooling rate is 41°C / s, and the water pressure is controlled at 0.38MPa. In the second stage, the cooling rate is 21°C / s.

[0049] (6) Coiling: The coiling temperature is 539°C and the coil is air-cooled to room temperature.

[0050] Example 2-3

[0051] A high-toughness hot-rolled steel strip with a yield strength of 600 MPa, the chemical composition of the steel billet is shown in Table 1, the production steps are the same as those in Example 1, and the differences in specific parameters during the production process from those in Example 1 are shown in Tables 2 and 3.

[0052] Comparative Examples 1-7

[0053] A hot-rolled steel strip, the chemical composition of the steel billet is shown in Table 1, and the differences in specific parameters during the production process from Example 1 are shown in Tables 2 and 3.

[0054] Table 1 Chemical composition of steel billets of various embodiments and comparative examples (wt.%)

[0055] project C Si Mn P S Al Ti Nb Cr N Example 1 0.073 0.25 1.64 0.014 0.0030 0.033 0.063 0.055 0.15 0.0037 Example 2 0.098 0.22 1.68 0.012 0.0020 0.034 0.066 0.058 0.17 0.0029 Example 3 0.082 0.25 1.63 0.013 0.0030 0.044 0.064 0.054 0.14 0.0030 Comparative Example 1 0.086 0.24 1.67 0.012 0.0026 0.040 0.059 0.062 0.11 0.0028 Comparative Example 2 0.062 0.17 1.80 0.015 0.0051 0.027 0.087 0.042 0.04 0.0046 Comparative Example 3 0.077 0.19 1.54 0.010 0.0019 0.029 0.079 0.038 0.02 0.0049 Comparative Example 4 0.074 0.18 1.73 0.009 0.0016 0.030 0.068 0.052 0.20 0.0034 Comparative Example 5 0.087 0.23 1.67 0.011 0.0031 0.041 0.043 0.072 0.01 0.0025 Comparative Example 6 0.075 0.22 1.71 0.013 0.0022 0.034 0.059 0.060 0.16 0.0031 Comparative Example 7 0.071 0.24 1.66 0.010 0.0017 0.038 0.068 0.051 0.12 0.0032

[0056] Table 2 Main process parameters of steelmaking in various embodiments and comparative examples

[0057]

[0058]

[0059] Table 3 Main process parameters of hot rolling in various embodiments and comparative examples

[0060]

[0061] In Comparative Example 1, process parameters such as superheat, continuous casting cooling water ratio and cooling rate, R2DT, FET, FDT, reduction ratio of the last pass of finishing rolling, MTI, first stage cooling rate, coiling temperature, etc. are different from those of the technical solution of the present invention.

[0062] In Comparative Example 2, the component contents of C, Mn, S, Cr, Nb, Ti, and N are different from those in the technical solution of the present invention, and the process parameters are all within the scope of the technical solution of the present invention.

[0063] In Comparative Example 3, the composition contents of Mn, Nb, Ti, and N are different from those in the technical solution of the present invention, and the process parameters such as holding time, soft blowing time, pulling speed, continuous casting cooling water ratio and cooling rate, intermediate billet thickness, FET, last pass reduction rate of finishing rolling, MTI, first stage cooling rate, CT, etc. are different from those in the technical solution of the present invention.

[0064] In Comparative Example 4, the component contents are all within the scope of the technical solution of the present invention, but the process parameters such as superheat, continuous casting cooling water ratio, cooling rate, CT, etc. are different from those of the technical solution of the present invention.

[0065] In Comparative Example 5, the contents of components such as Cr, Nb, and Ti are different from those in the technical solution of the present invention, and the process parameters such as R2DT and FDT are different from those in the technical solution of the present invention.

[0066] In Comparative Example 6, the component contents are all within the scope of the technical solution of the present invention, and the process parameters such as FDT, last pass reduction rate, MT1, first stage cooling rate, etc. are different from the technical solution of the present invention.

[0067] In Comparative Example 7, the contents of components such as Nb and Ti are different from those in the technical solution of the present invention, and the process parameters such as FDT, MT1, first-stage cooling rate, and CT are different from those in the technical solution of the present invention.

[0068] The mechanical properties of the hot-rolled steel strips obtained in the embodiments and comparative examples are shown in Table 4.

[0069] Table 4 Mechanical properties of hot rolled strip steel obtained in Examples 1-3 and Comparative Examples 1-7

[0070]

[0071] The microstructure of the hot rolled strip in Example 1-3 is shown in FIG. Figure 1-Figure 3 As shown, the microstructure of the hot-rolled strip in Comparative Example 3-4 is as shown in Figure 4-Figure 5As shown. It can be seen that the microstructure of the hot-rolled steel strip in Examples 1-3 is mainly polygonal ferrite + acicular ferrite, with uniform and fine grains and a grain size of ≥12; the microstructure of the hot-rolled steel strip in Comparative Example 3 is mainly polygonal ferrite, with an uneven structure and coarse grains; the microstructure of the hot-rolled steel strip in Comparative Example 4 is mainly ferrite + pearlite, with an uneven structure, coarse grains, and a large size of precipitated phase, which can be seen under a metallographic microscope.

[0072] By comparing Examples 1-3 and Comparative Examples 1-7, it can be seen that the 12-16 mm hot-rolled strip steel produced according to the composition and process of the present invention has strong low-temperature impact toughness at -20°C and -40°C on the basis of yield strength meeting the 600 MPa grade. However, due to differences in composition, process, etc., the microstructure, strength, and toughness indicators of the comparative examples are not ideal, and it is difficult to meet the application requirements in the field of engineering machinery.

[0073] Although the present invention has been described in detail with reference to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention.

Claims

1. A method for producing a high-toughness hot-rolled steel strip with a yield strength of 600 MPa, comprising the steps of smelting, continuous casting, heating, rolling, cooling and coiling, characterized in that: The chemical composition and mass percentage of the steel billet are respectively C: 0.07%-0.10%, Si: 0.15%-0.30%, Mn: 1.60%-1.75%, P≤0.018%, S≤0.0040%, Ti: 0.055%-0.070%, Nb: 0.050%-0.065%, Cr: 0.10%-0.20%, Al: 0.020%-0.050%, N≤0.0040%, and the rest are Fe and unavoidable impurities; Among them, the whole process of continuous casting adopts argon protection pouring, low superheat and constant pulling speed control, the superheat is 15-25℃, and the casting speed is 1.0-1.2m / min; The AlowC intercooling mode is used for cooling in the continuous casting process, the secondary cooling water volume is 0.80-0.90L / kg, the cooling rate is controlled at 7-9℃ / s, and the continuous casting billet thickness is 230mm; The rolling process is divided into rough rolling and finishing rolling. The final rolling temperature of rough rolling is 1040-1080℃. Five round-trip rolling is adopted to obtain the intermediate billet. The thickness of the intermediate billet is 46-56mm. The entrance temperature of finishing rolling is 1000-1030℃. The final rolling temperature of finishing rolling is 830-870℃. The reduction rate of the last pass of finishing rolling is ≥14%. The thickness of the strip after 7 passes of finishing rolling is 12-16mm. The cooling process adopts two-stage water cooling. The cooling rate of the first stage is 30-45℃ / s, the cooling outlet temperature is 660-700℃, and the water pressure is controlled at 0.38-0.42MPa; the cooling rate of the second stage is 15~25℃ / s; The thickness of the steel strip is 12-16 mm, the yield strength is 600-700 MPa, the tensile strength is 700-800 MPa, the elongation is >20%, and the impact energy at -40°C is >180 J.

2. The production method according to claim 1, characterized in that The smelting process adopts LF+RH double refining process, titanium-iron alloy is added to the RH furnace, the vacuum pressure holding time is ≥12min, the pure degassing time is ≥7min, and the soft blowing time is ≥12min.

3. The production method according to claim 1, characterized in that In the heating process, the temperature of the soaking section is 1220-1260°C, the soaking time is 30-60min, the temperature out of the heating furnace is 1200-1240°C; the total heating time in the furnace is 180-260min.

4. The production method according to claim 1, characterized in that In the coiling process, the coiling temperature is 510-540°C, and after coiling, the coil is air-cooled to room temperature.

Citation Information

Patent Citations

  • A hot-rolled coil of Q550E high-strength steel and its production method

    CN104831167B

  • Low-cost Ti microalloyed 620 MPa-grade hot rolled steel belt and production method

    CN110306124A

  • A method for improving the low-temperature impact toughness of thick-gauge high-strength steel

    CN112828036B

  • High intensity steel plate and preparation method thereof

    CN101451212A

  • Steel plate with low welding crack sensitivity and manufacturing method thereof

    CN105441790A