A method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursor

By using hydrogel precursor ink combined with aluminum dihydrogen phosphate and ceramic powder in traditional light-curing 3D printing technology, the problems of powder settlement and sintering shrinkage are solved, and high-precision and low-shrinkage ceramic preparation is achieved. Suitable for aerospace applications with complex structures.

CN116462492BActive Publication Date: 2024-10-01LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310496225.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-10-01
Estimated Expiration
2043-05-05

AI Technical Summary

Technical Problem

Traditional light-curing 3D printing ceramic technology has problems with powder settlement and large-scale shrinkage during the sintering process, resulting in poor printing accuracy and structural deformation, making it difficult to meet the high-precision needs of aerospace and other fields.

Method used

Aluminum dihydrogen phosphate is used as an inorganic binder and combined with ceramic powder to prepare a photosensitive 3D printing hydrogel precursor ink. A covalently cross-linked hydrogel skeleton is formed through photocuring technology, combined with high-temperature sintering to reduce shrinkage. .

Benefits of technology

It achieves high precision and low shrinkage in the ceramic printing process, avoids powder settlement and structural collapse after sintering, provides higher formability and plasticity, and reduces the linear shrinkage of ceramics to about 10%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116462492B_ABST
    Figure CN116462492B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing low-shrinkage ceramics by photocuring 3D printing hydrogel precursors, comprising: preparing photosensitive hydrogel precursor ink, establishing a three-dimensional printing structure, using photocuring 3D printing technology to obtain a three-dimensional structured hydrogel precursor green body, and then preparing low-shrinkage ceramics by high-temperature sintering. The hydrogel precursor ceramics obtained by the preparation method of the present invention have the advantages of high-precision printing, structural diversity, low shrinkage, etc., and can provide a new method for the design and preparation of high-precision complex structure ceramics in the fields of high-end equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a method for preparing low-shrinkage ceramics by using a photocurable 3D printing hydrogel precursor. Background Art

[0002] Ceramics are widely used in catalyst carriers, sensor materials, purification and separation fields due to their advantages such as high hardness, thermal shock resistance, high chemical stability, high temperature resistance and good mechanical properties. Especially for the core components in the aerospace field, which need to be able to withstand problems such as bad weather, high temperature and high pressure, and complex environment, ceramics are undoubtedly the best choice, and such applications have strict requirements on the dimensional accuracy, high temperature performance and structural complexity of parts. However, the ceramic processing technology itself is relatively complex, and traditional ceramic processing technologies such as hot pressing technology have the disadvantages of long processing technology cycle, low efficiency, difficulty in forming complex structures, low precision and rough surface. As a result, the development of high-precision ceramics is increasingly restricted, and it is extremely unfavorable for its development in precision fields such as aerospace. However, in recent years, the emerging light-curing 3D printing technology has made up for the shortcomings of traditional ceramic manufacturing injection molding. As an efficient, low-cost and multifunctional additive manufacturing technology, light-curing 3D printing technology can accurately construct complex and high-precision three-dimensional models, so it can be widely used in the precision field to build complex ceramic structures. However, traditional light-curing 3D printing ceramic technology generally uses photosensitive resin to support molding, so it can be widely used in the precision field to build complex ceramic structures. However, traditional photocuring 3D printing ceramic technology generally uses photosensitive resin to support molding. During the preparation process, there are usually problems with powder sedimentation, and large-scale shrinkage will occur during the sintering process. Due to the heterogeneous structures of each phase formed layer by layer, it will cause uneven heating during the debinding and sintering process, resulting in shrinkage and deformation.

[0003] A porous ceramic used in a portable Chinese herbal medicine atomizer and a manufacturing method thereof, application number CN115259891A, adopts the traditional cold isostatic pressing method to prepare the porous ceramic used in the Chinese herbal medicine atomizer, which solves the technical problem that the traditional porous ceramic is not suitable for the atomization of Chinese herbal medicine. It invented a porous ceramic suitable for the atomization of Chinese herbal medicine, which improves the oil storage effect and oil locking effect of the porous ceramic. Aluminum dihydrogen phosphate is only one of the selected binders, and the porous ceramic system includes adhesives, pore-forming agents, ceramic powders, etc.

[0004] The invention name is 3D printed MOFs particle network hydrogel and its preparation method and application, and the application number is CN202211269778. It discloses mixing polyvinyl alcohol aqueous solution, sodium carboxymethyl cellulose and MOFs organic ligand to obtain hydrogel ink; performing direct writing 3D printing on the hydrogel ink to obtain a 3D printed hydrogel structure containing MOFs organic ligands; freezing and thawing the 3D printed hydrogel structure containing MOFs organic ligands in sequence to obtain a 3D printed hydrogel reinforcement structure; soaking the 3D printed hydrogel reinforcement structure in a metal salt organic solution and performing water exchange equilibrium to obtain the 3D printed soft hydrogel, and the material presents sub-millimeter resolution and high shape fidelity. The material targeted by this invention is hydrogel, and the direct writing 3D printing technology is used. Summary of the invention

[0005] The purpose of the present invention is to solve the defects of the above-mentioned prior art and provide a method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursor, which overcomes the problems caused by ink preparation and sintering in the existing photocuring 3D printing ceramic technology.

[0006] The preparation of ceramics with photocurable 3D printed hydrogel precursors can effectively solve the problems of printing accuracy, dimensional shrinkage and deformation of ceramics. In terms of printing, aluminum dihydrogen phosphate combines with ceramic powder more evenly, and there will be no sedimentation in the resin. Aluminum dihydrogen phosphate contains a certain amount of water during the preparation process, and can also combine with hydrogel unsaturated monomers, providing good photocuring performance for ceramic printing. In terms of sintering, unlike traditional photocurable 3D printed ceramics, after sintering, the resin decomposition causes a large amount of shrinkage or even collapse of the ceramic structure. The inorganic binder of aluminum dihydrogen phosphate serves as the ceramic skeleton, and only a small part of the organic material is decomposed by heat. Therefore, the method of preparing low-shrinkage ceramics with photocurable 3D printed hydrogel precursors of the present invention mainly solves these two problems.

[0007] The present invention adopts the following technical solution:

[0008] A method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursors comprises the following steps:

[0009] Dissolving ceramic powder, inorganic non-metallic adhesive, unsaturated monomer, aqueous photoinitiator, crosslinking agent, and light absorber (dye) in a solvent to prepare photosensitive 3D printing hydrogel precursor ceramic ink;

[0010] Using software 3D modeling, photosensitive 3D printing hydrogel precursor ceramic ink is placed into the material tank for light-curing 3D printing to obtain a printed ceramic structure;

[0011] The printed ceramic green body is placed at room temperature to dry and remove water, degreased at medium-high temperature, and sintered at high temperature to form a ceramic structure.

[0012] Preferably, the ceramic powder is one of Al2O3 ceramic powder (particle size 20-100nm), SiO2 ceramic powder (particle size 20-100nm), and TiO2 ceramic powder (particle size 20-100nm).

[0013] Preferably, the mass of the ceramic powder is 40%-60% of the total components.

[0014] Preferably, the inorganic non-metallic binder is aluminum dihydrogen phosphate sol binder.

[0015] Preferably, the mass of the aluminum dihydrogen phosphate sol binder is 30%-40% of the total components.

[0016] Preferably, the unsaturated monomer is one or two of acrylamide, hydroxyethyl acrylamide, dimethyl acrylamide, N-isopropyl acrylamide, acrylic acid, and N-vinyl pyrrolidone.

[0017] Preferably, the mass of the unsaturated monomer is 10%-20% of the total components.

[0018] Preferably, the aqueous initiator is one of LAP, V-50, BAPO-ONa, BAPO-OLi, and PEG-BAPO.

[0019] Preferably, the preparation method of the aluminum dihydrogen phosphate sol adhesive is: add 1 mol Al(OH)3 to 3.5 mol of a 10.4 mol / L phosphoric acid solution, stir at 100°C until it becomes colorless and transparent, and the obtained aluminum dihydrogen phosphate adhesive is obtained.

[0020] Preferably, the photoinitiator is 0.1%-1% of the mass of the unsaturated monomer.

[0021] Preferably, the cross-linking agent is one of N,N-methylenebisacrylamide, polyethylene glycol diacrylate, and a urea-based cross-linking agent containing a double bond.

[0022] Preferably, the mass of the cross-linking agent is 0.2%-2% of the mass of the unsaturated monomer.

[0023] Preferably, the light absorber is one of tartrazine, riboflavin, 2-hydroxy-4-n-octyloxybenzophenone, and 2-2(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole.

[0024] Preferably, the mass of the light absorber is 1‰-5‰ of the total components.

[0025] Preferably, the light-curing 3D printing parameters are: the wavelength of the light source is 385-405 nm; the intensity of the light source is 500-800 mW; the single-layer exposure time is 10-30 s; and the single-layer slice thickness is 0.02-0.1 mm.

[0026] Preferably, the sintering parameters of the photocurable 3D printed hydrogel precursor for preparing low shrinkage ceramics are as follows: during the dehydration process, the printed green body is dried at room temperature for one week, dried at 70°C for one week, heated to 100°C for one week, and dried at 200°C for one week to remove crystal water; during the degreasing process: 1°C min -1 The heating rate is 100°C and the temperature is kept at 300°C for 10 hours. Then the temperature is kept at 500°C for 10 hours to completely remove the organic matter. The sintering process is: -1 The temperature was raised to 800°C at a rate of 1000 °C and then naturally cooled as the furnace cooled after 2 hours of calcination.

[0027] Beneficial effects of the present invention:

[0028] Compared with the prior art, the present invention has the following advantages:

[0029] 1. The photocurable 3D printing hydrogel precursor ceramic prepared by the present invention can be deformed and stretched and has plasticity.

[0030] 2. The photocurable 3D printing hydrogel precursor ceramic prepared by the present invention will not separate from the powder and the solvent during the printing process, and has higher fusion properties.

[0031] 3. Compared with traditional photocurable 3D printed resin-based ceramics, the photocurable 3D printed hydrogel precursor ceramics prepared by the present invention have lower shrinkage and better formability after sintering.

[0032] 4. The ceramic linear shrinkage of the present invention is about 10%. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the preparation process of the present invention;

[0034] Figure 2 This is a diagram showing the flexibility of the hydrogel precursor of Example 1 of the present invention;

[0035] Figure 3 This is a high-precision physical picture of the ceramic of Example 2 of the present invention;

[0036] Figure 4 This is a diagram showing the low shrinkage of the ceramic of Example 3 of the present invention. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0039] The present invention provides a method for preparing low-shrinkage ceramics by photocuring 3D printing hydrogel precursors. The main steps are as follows: ceramic powder, aluminum dihydrogen phosphate adhesive, unsaturated monomers, aqueous photoinitiators, and light absorbers (dye) are fully mixed to prepare photosensitive hydrogel precursor ceramic ink, a three-dimensional structure model is established by software, the hydrogel precursor ceramic ink is placed in a material box, and photocuring 3D printing is performed under set 3D printing parameters to prepare a flexible ceramic precursor of a covalently cross-linked hydrogel skeleton, which can realize photocuring printing of low-shrinkage ceramics and provide a manufacturing method for low-shrinkage ceramics with complex structures.

[0040] The present invention provides a method for preparing low-shrinkage ceramics by using a photocurable 3D-printed hydrogel precursor, comprising the following steps: fully mixing ceramic powder, aluminum dihydrogen phosphate adhesive, unsaturated monomer, aqueous photoinitiator, and light absorber (dye) components to prepare photosensitive hydrogel ceramic ink, establishing a three-dimensional structure model by using software, putting the hydrogel ceramic ink into a material box, performing photocurable 3D printing under set 3D printing parameters to prepare a flexible ceramic precursor of a covalently cross-linked hydrogel skeleton, and preparing low-shrinkage structurally diversified ceramics through high-temperature sintering.

[0041] The present invention proposes a hydrogel water-based ceramic ink for the first time, realizes the preparation of flexible ceramic precursors, and realizes low-shrinkage photocurable ceramics after sintering. This method provides theoretical support for photocuring printing of low-shrinkage complex structure ceramics.

[0042] like Figure 1 As shown, a method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursor of the present invention comprises the following steps:

[0043] The ceramic powder, aluminum dihydrogen phosphate adhesive, unsaturated monomer, aqueous photoinitiator, crosslinking agent, and light absorber (dye) components are fully mixed to prepare photosensitive hydrogel ceramic ink;

[0044] The software is used to build a three-dimensional structural model, the hydrogel ceramic ink is placed in the material box, and the photocuring 3D printing is performed under the set 3D printing parameters to prepare a covalently cross-linked hydrogel-supported flexible ceramic precursor;

[0045] The photocurable 3D printed hydrogel precursor green body was dried at room temperature, low-temperature dried at 70°C, degreased at medium and high temperatures, and then sintered at high temperature to produce low-shrinkage structurally diversified ceramics.

[0046] Furthermore, the ceramic powder is one of alumina ceramics, silicon dioxide ceramics and titanium dioxide ceramics.

[0047] Furthermore, the mass of the ceramic powder accounts for 40%-60% of the mass of the total components, more preferably 40%-55%, and most preferably 45%-50%.

[0048] Furthermore, the unsaturated monomer is one or two of acrylamide, hydroxyethyl acrylamide, dimethyl acrylamide, N-isopropyl acrylamide, acrylic acid, and N-vinyl pyrrolidone.

[0049] Furthermore, the mass of aluminum dihydrogen phosphate accounts for 30%-40% of the total component mass, more preferably 30%-38%, and most preferably 35%-38%.

[0050] Furthermore, the mass of the unsaturated monomer accounts for 10%-20% of the mass of the total components, more preferably 12%-20%, and most preferably 15%-18%.

[0051] In the present invention, the aqueous photoinitiator is preferably one of LAP, V-50, BAPO-ONa, BAPO-OL i, and PEG-BAPO.

[0052] Furthermore, the mass of the aqueous photoinitiator is preferably 0.1%-1% of the mass of the unsaturated monomer; more preferably 0.3%-0.8%, and most preferably 0.5%-0.7%.

[0053] In the present invention, the cross-linking agent is preferably one of N,N-methylenebisacrylamide, polyethylene glycol diacrylate, and a urea-based cross-linking agent containing a double bond.

[0054] Furthermore, the mass of the cross-linking agent is preferably 0.2%-2% of the mass of the unsaturated monomer; more preferably 0.5%-1.5%; most preferably 0.8%-1.2%.

[0055] In the present invention, the light absorber is one of tartrazine, riboflavin, 2-hydroxy-4-n-octyloxybenzophenone and 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole.

[0056] Preferably, the mass of the light absorber is 1‰-5‰ of the mass of the total components; more preferably, 1.5‰-4.5‰; most preferably, 3‰-4‰.

[0057] In the present invention, the parameters of photocuring 3D printing are: the wavelength of the light source is preferably 385-405 nm; the intensity of the light source is preferably 500-800 mW; the exposure time of a single layer is preferably 10-20 s; and the thickness of a single layer slice is preferably 0.05-0.2 mm.

[0058] In the present invention, the sintering temperature parameters of the photocurable 3D printed ceramics are: the printed green body is air-dried at room temperature for one week, heated at a low temperature of 70°C for one week, heated to 100°C for one week, and dried at 200°C for one week to remove the crystal water. Degreasing process: 1°C min -1 The heating rate is 100°C and the temperature is kept at 300°C for 10 hours. Then the temperature is kept at 500°C for 10 hours to completely remove the organic matter. The sintering process is: -1 The temperature was raised to 800°C at a rate of 1000 °C and then naturally cooled as the furnace cooled after 2 hours of calcination.

[0059] Example 1

[0060] 30.40g alumina ceramic powder, 20g aluminum dihydrogen phosphate sol, 8.0g acrylamide, 0.66g acrylic acid, 0.34g polyethylene glycol diacrylate and 0.17g aqueous photoinitiator LAP, and 5 drops of lemon yellow were used to prepare photosensitive 3D printing hydrogel ceramic ink. A three-dimensional metamaterial structure model was established using software. The photosensitive 3D printing hydrogel ink was placed in a material tank. The 3D printing parameters were as follows: light source wavelength 405nm; light source intensity 800mW; single layer exposure time 15s; single layer slice thickness preferably 0.05mm, so as to obtain a covalently cross-linked flexible precursor hydrogel ceramic structure.

[0061] like Figure 2 As shown, it can be seen that the hydrogel precursor has good flexibility.

[0062] Example 2

[0063] 30.40g alumina ceramic powder, 20g aluminum dihydrogen phosphate sol, 8.0g acrylamide, 0.66g acrylic acid, 0.34g polyethylene glycol diacrylate and 0.17g aqueous photoinitiator LAP, 5 drops of lemon yellow were used to prepare photosensitive 3D printing hydrogel ceramic ink, a three-dimensional metamaterial structure model was established using software, the photosensitive 3D printing hydrogel ink was put into a material tank, and photocuring 3D printing was performed under the following 3D printing parameters: light source wavelength 405nm; light source intensity 800mW; single layer exposure time 15s; single layer slice thickness preferably 0.05mm to obtain a covalently cross-linked flexible precursor hydrogel ceramic structure, the printed green body was dried at room temperature for one week, heated at low temperature 70℃ for one week, heated to 100℃ for one week, dried at 200℃ for one week to remove crystal water, and the degreasing process: 1℃min -1 The heating rate is 100°C and the temperature is kept at 300°C for 10 hours. Then the temperature is kept at 500°C for 10 hours to completely remove the organic matter. The sintering process is: -1 The temperature was raised to 800°C at a rate of 100°C and then naturally cooled with the furnace after 2 hours of calcination to obtain light-cured 3D printed ceramics.

[0064] like Figure 3 As shown, it can be seen that the hydrogel precursor ceramic has high-precision printability.

[0065] Example 3

[0066] 30.40g alumina ceramic powder, 20g aluminum dihydrogen phosphate sol, 8.0g acrylamide, 0.66g acrylic acid, 0.34g polyethylene glycol diacrylate and 0.17g aqueous photoinitiator LAP, 5 drops of lemon yellow were used to prepare photosensitive 3D printing hydrogel ceramic ink. A three-dimensional metamaterial structure model was established using software. The photosensitive 3D printing hydrogel ink was placed in a material tank. The photocuring 3D printing was performed under the following 3D printing parameters: light source wavelength 405nm, light source intensity 800mW; single layer exposure time 15s; single layer slice thickness preferably 0.05mm to obtain a covalently cross-linked flexible precursor hydrogel ceramic structure. The printed green body was dried at room temperature for one week, heated at low temperature 70℃ for one week, heated to 100℃ for one week, and dried at 200℃ for one week to remove crystal water. The degreasing process: 1℃min -1 The heating rate is 100°C and the temperature is kept at 300°C for 10 hours. Then the temperature is kept at 500°C for 10 hours to completely remove the organic matter. The sintering process is: -1 The temperature was raised to 800°C at a rate of 100°C and then naturally cooled with the furnace after 2 hours of calcination to obtain light-cured 3D printed ceramics.

[0067] like Figure 4 As shown, it can be seen that the hydrogel precursor ceramic has a low shrinkage rate.

[0068] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursors. Features , including the following steps: Step 1. Fully mix ceramic powder, aluminum dihydrogen phosphate adhesive, unsaturated monomer, water-based photoinitiator, crosslinker, and light absorber components to prepare photosensitive hydrogel ceramic ink, wherein the mass of ceramic powder accounts for 40%-60% of the total mass of the components, the mass of aluminum dihydrogen phosphate accounts for 30%-40% of the total mass of the components, the mass of unsaturated monomer accounts for 10%-20% of the total mass of the components, the mass of the water-based photoinitiator is 0.1%-1% of the mass of the unsaturated monomer, the mass of the crosslinker reagent is 0.2%-2% of the mass of the unsaturated monomer, and the mass of the light absorber is 1‰-5‰ of the mass of the total components, and the sum of the contents of the above components is 100%; Step 2. Use software to build a three-dimensional structure model, put the hydrogel ceramic ink into the material box, and perform photocuring 3D printing under the set 3D printing parameters to prepare a covalently cross-linked hydrogel flexible ceramic precursor; Step 3. Dry the photocurable 3D printed hydrogel precursor green body at room temperature, dry it at 70°C, degrease it at medium or high temperature, and prepare a low shrinkage structure diversified ceramic by high temperature sintering; The sintering temperature parameters of the photocurable 3D printed ceramics are as follows: the printed green body is dried at room temperature for one week, heated at a low temperature of 70°C for one week, heated to 100°C for one week, and dried at 200°C for one week to remove the crystal water; Degreasing process: 1℃min -1 The heating rate is 1℃min, and the temperature is kept at 300℃ for 10 hours. Then the temperature is kept at 500℃ for 10 hours to completely remove the organic matter. The sintering process is 1℃min -1 The temperature was raised to 800°C at a rate of 1000 °C and then naturally cooled as the furnace cooled after 2 hours of calcination.

2. The method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursor according to claim 1, It is characterized in that Step 1, the ceramic powder is one of alumina ceramics, silicon dioxide ceramics, and titanium dioxide ceramics.

3. The method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursor according to claim 2, It is characterized in that The particle size of alumina ceramic powder is 20-200nm; the particle size of silicon dioxide ceramic powder is 20-200nm; the particle size of titanium dioxide ceramic powder is 20-200nm.

4. The method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursor according to claim 1, It is characterized in that Step 1, the unsaturated monomer is one or two of acrylamide, hydroxyethyl acrylamide, dimethyl acrylamide, N-isopropyl acrylamide, acrylic acid, and N-vinyl pyrrolidone.

5. The method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursor according to claim 1, It is characterized in that Step 1, the aqueous photoinitiator is one of LAP, V-50, BAPO-ONa, BAPO-OLi, and PEG-BAPO.

6. The method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursor according to claim 1, It is characterized in that The crosslinking agent is one of N,N-methylenebisacrylamide, polyethylene glycol diacrylate, and a urea-based crosslinking agent containing a double bond.

7. The method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursor according to claim 1, It is characterized in that In step 1, the light absorber is one of tartrazine, riboflavin, 2-hydroxy-4-n-octyloxybenzophenone, and 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole.

8. The method for preparing low shrinkage ceramics by photocuring 3D printing hydrogel precursor according to claim 1, It is characterized in that Step 2: The parameters of light-curing 3D printing are: the wavelength of the light source is 385-405nm; the light source intensity is 500-800mW; the single layer exposure time is 10-20s; The thickness of single-layer slices is 0.05-0.2 mm.

9. A low shrinkage ceramic prepared by photocuring 3D printing hydrogel precursor, It is characterized in that The method for preparing low shrinkage ceramics by using a photocurable 3D printing hydrogel precursor as described in any one of claims 1 to 8 is obtained.