A method for producing low-calcium salt from calcium sulfate brine
The calcium sulfate type brine process is used to remove calcium and magnesium impurities in lithium battery production, reduce the sulfate ion content, solve the problem of high quality requirements for raw material salt in lithium battery production, realize the production of high-quality low-calcium sodium chloride, and avoid food Safety incidents and additional equipment construction, suitable for low-cost calcium chloride acquisition.
Patent Information
- Application Number
- CN202310548546.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-05-16
AI Technical Summary
In the existing lithium battery production process, the special sodium carbonate raw material salt for lithium carbonate has high quality requirements, but the existing salt brine production process cannot meet the requirements, resulting in increased investment and equipment requirements, and the traditional process is difficult to control during the sulfate removal process. May cause food safety accidents.
The calcium sulfate type brine process is used to remove calcium and magnesium impurities in the brine through the two-alkali method. After evaporation, concentration and washing, calcium chloride is added to precipitate sodium sulfate, reducing the sulfate ion content, and returned to the brine system for reuse, simplifying the process and avoiding Construction of additional equipment.
It achieves high-quality extraction of low-calcium sodium chloride products. The total calcium and magnesium ions are reduced to less than 70ppm, and the sulfate ion content is reduced to less than 0.30%. Food safety accidents and additional equipment construction are avoided. The operation is simple and suitable for low-cost acquisition of chlorine. The situation of calcium chloride.
Smart Images

Figure CN116477643B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of inorganic chemical industry and relates to a method for producing low-calcium salt, in particular to a method for producing low-calcium salt from calcium sulfate type brine. Background Art
[0002] Currently, lithium batteries are developing rapidly in the world, and the demand for lithium batteries at home and abroad is also increasing. However, the special sodium carbonate used to produce lithium carbonate has high requirements on the quality of raw salt. The current brine production process cannot meet its requirements. The market has proposed to use gypsum brine to produce sodium carbonate by co-producing salt and saltpeter. However, this method will increase the site and equipment for saltpeter production, and increase a lot of investment. Summary of the invention
[0003] The object of the present invention is to provide a method for producing low-calcium salt from calcium sulfate type brine. In this method, refined brine is obtained by adding soda ash and caustic soda to the original brine to remove impurities such as calcium and magnesium, and the refined brine is evaporated and concentrated to a point close to the NaCl-Na2SO4 saturation point, and the crystallized salt is collected, washed with the refined brine, dehydrated and dried to obtain the product salt, and the mother liquor of salt production is added with calcium chloride to precipitate sodium sulfate, and then returned to the brine pretreatment system for repeated use. The process is simple and has great practical value in places where calcium chloride can be obtained at a low cost.
[0004] In order to achieve the above invention object, the specific technical solution of the present invention is:
[0005] A method for producing low-calcium salt from calcium sulfate type brine, comprising the following steps:
[0006] Gypsum-type brine is used as raw material, and the raw material is passed into a pretreatment reaction tank. The calcium and magnesium content in the brine is first removed to less than 15 mg / L through a two-alkali method, and then the precipitated material is filtered; the obtained clear liquid is pumped into an evaporation salt-making device, and vacuum evaporated and concentrated at a certain temperature to obtain salt slurry and evaporation mother liquor respectively; the salt slurry is washed with refined brine, and then dehydrated and dried to obtain a low-calcium salt product; a calcium chloride solution is added to the evaporation mother liquor to reduce the sulfate concentration in the mother liquor, and after the reaction is completed, the clear liquid is returned to the pretreatment reaction tank, the precipitated material is filtered, and the filtrate is returned to the mother liquor pool for storing the evaporation mother liquor, and the gypsum residue is landfilled.
[0007] As a better implementation of the present application, the two alkalis in the two-alkali method are caustic soda and soda ash; the specific steps of removing the calcium and magnesium content in the brine to less than 15 mg / L by the two-alkali method are:
[0008] Sodium carbonate is first passed into the gypsum-type brine to remove calcium, and then sodium hydroxide is used to adjust the pH of the brine. After the reaction is completed, the clear liquid and the precipitate are separated by filtration. The filter residue after filtration is calcium-magnesium sludge, which can be used as engineering landfill.
[0009] As a better embodiment of the present application, the amount of sodium carbonate added is carried out according to the molar ratio of calcium + strontium to sodium carbonate of 1:1.05-1.15; sodium hydroxide is used to adjust the pH value of the brine to 11.0-12.0; these two conditions are preferably a molar ratio of (calcium + strontium) to sodium carbonate of 1:1, and a pH of 12; a molar ratio of (calcium + strontium) to sodium carbonate of 1:1.05, and a pH of 12; a molar ratio of (calcium + strontium) to sodium carbonate of 1:1.1, and a pH of 11.5; a molar ratio of (calcium + strontium) to sodium carbonate of 1:1.1, and a pH of 12; a molar ratio of (calcium + strontium) to sodium carbonate of 1:1.15, and a pH of 11.5; a molar ratio of (calcium + strontium) to sodium carbonate of 1:1.15, and a pH of 12. More preferably, the amount of sodium carbonate added is based on a molar ratio of calcium + strontium to sodium carbonate of 1:1.1; sodium hydroxide is used to adjust the pH value of the brine to 11.5.
[0010] Furthermore, after the filter press is completed, the pH of the clear liquid is adjusted to 7.8-8.2.
[0011] As a better implementation mode in the present application, the temperature of vacuum evaporation concentration is 50°C-110°C, specifically 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, etc.; the vacuum evaporation concentration multiple is 8-11 times, specifically 8 times, 9 times, 10 times or 11 times, etc.
[0012] As a better implementation method in the present application, after the vacuum evaporation concentration is completed, the salt slurry is washed with refined brine, and the salt slurry is washed according to the washing water volume of V washing water: V salt slurry = 1-2:1.
[0013] As a better implementation method in the present application, the calcium chloride-containing solution is a calcium chloride solution, polysilicon wastewater containing calcium chloride, or a mixture of the above two substances; in the calcium chloride-containing solution, CaCl2 is added to the evaporated mother liquor according to the molar ratio of sulfate to calcium chloride = 1:1.06-1.14.
[0014] As a better implementation method in the present application, in the low-calcium salt product, the total amount of calcium and magnesium ions is reduced to below 70 ppm, and the sulfate ion content is reduced to below 0.30%.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) Extract qualified low-calcium sodium chloride products from calcium sulfate brine through a simple process.
[0017] (ii) This process can reduce the total amount of calcium and magnesium ions in industrial wet salt and industrial dry salt to below 70 ppm, and also reduce the sulfate ion content in the salt to below 0.30%.
[0018] (III) At present, the gypsum brine salt production process is generally divided into three categories: ① Salt production - barium sulfate removal ② Salt production - calcium sulfate removal ③ Salt and nitrate co-production. This process avoids the food safety accidents caused by the traditional process in the process of sulfate removal due to the extremely difficult control of the amount of barium added; it also avoids the salt and nitrate co-production. Although it can use the different solubility of sodium chloride and sodium sulfate with temperature to achieve salt and nitrate separation, it requires the construction of nitrate evaporation equipment, dehydration and drying equipment and packaging lines, etc., and the return of nitrate mother liquor to salt will increase the difficulty and benefits of salt production operations; the calcium sulfate removal process can greatly avoid the occurrence of food safety accidents, and at the same time does not require the construction of additional evaporation equipment, etc., it is simple to operate, and it can also reduce the sulfate in the salt to below 0.30%, which is very important for Ca 2+ Where it can be obtained at low cost, there are great advantages. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The present invention provides a schematic diagram of the process for producing low-calcium salt from calcium sulfate brine. DETAILED DESCRIPTION
[0020] In order to make the content of the present invention easier to understand, the process described in the present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following embodiments.
[0021] The composition of the gypsum-based brine in the following examples is shown in Table 1.
[0022] Table 1 Reference ingredients of raw materials
[0023]
[0024]
[0025] In the following embodiments, the wash water is refined brine, and the refined brine index is shown in the following table:
[0026] Ca Mg Cl <![CDATA[SO4 2- ]]> g / L g / L g / L g / L 0.010 0.004 168.4 3.87
[0027] In the present application, unless otherwise specified, all ratios involved are mass ratios; and % are mass percentages.
[0028] Embodiment 1:
[0029] The gypsum-type brine is decalcified according to the molar ratio of (calcium + strontium): sodium carbonate of 1:1.10, and then the pH of the brine is adjusted to 11.0 with sodium hydroxide. After the reaction is completed, the clear liquid is separated from the precipitate by filter pressing, and the pH of the clear liquid is reversely adjusted to 7.8, and then pumped into the evaporation tank, the evaporation temperature is controlled to 55°C, and the vacuum evaporation concentration multiple is 8 times. After the evaporation is completed, the salt slurry is washed with a wash water volume of V (wash water): V (salt slurry) of 2:1, and the washed salt slurry is dried and dehydrated to obtain a low-calcium salt product, and CaCl2 is added to the mother liquor according to the molar ratio of sulfate: calcium chloride of 1:1.06. After the reaction is completed, the precipitate is separated from the clear liquid by filter pressing, and the clear liquid is returned to the raw material pool; finally, the Ca in the low-calcium salt product is 2+ Mg 2+ , SO4 2- and Cl - The content of SO4 in the mother liquor after CaCl2 treatment was tested and the test results are shown in Table 2-1. 2- The content was tested, and the test results are shown in Table 2-2. According to the data results in Table 2-1 and Table 2-2, the total calcium and magnesium ions in industrial dry salt and wet salt are both below 70ppm, and the SO4 2- The content is 4.83g / L, close to 4.12g / L in the original brine. Both the salt product and the mother liquor meet the expected indicators.
[0030] Table 2-1 Low calcium salt data detection
[0031]
[0032] Table 2-2 Calcium chloride treatment mother liquor
[0033] Sulfate: Calcium Chloride Molar Ratio <![CDATA[Ca 2+ (g / L)]]> <![CDATA[Mg 2+ (g / L)]]> <![CDATA[SO4 2- (g / L)]]> <![CDATA[Cl - (g / L) <!-- 3 -->]]> 1:1.06 1.26 0 4.83 188
[0034] Comparison of traditional salt products and this process indicators
[0035]
[0036] Through the comparison table of traditional salt products and this process index, it can be clearly seen that this process can reduce the total amount of calcium and magnesium ions in industrial wet salt and industrial dry salt to below 70ppm, and also reduce the sulfate ion content in the salt to below 0.30%. At present, the gypsum-based brine salt-making process is roughly divided into three types: ① Salt-making-barium sulfate removal ② Salt-making-calcium sulfate removal ③ Salt and nitrate co-production. In the process of barium sulfate removal, the amount of barium added is extremely difficult to control, which is easy to cause food safety accidents; although the salt and nitrate co-production can use the different solubility of sodium chloride and sodium sulfate with temperature to achieve salt and nitrate separation, it is necessary to build nitrate evaporation equipment, dehydration and drying equipment and packaging lines, etc., and the return of nitrate mother liquor to salt will increase the difficulty and benefits of salt-making operations; the calcium sulfate removal process can avoid the occurrence of food safety accidents to a great extent, and does not require additional evaporation equipment, etc., the operation is simple, and the sulfate in the salt can also be reduced to below 0.30%, which is a great advantage for places where Ca2+ can be obtained at low cost.
[0037] Example 2
[0038] The gypsum-type brine is decalcified according to the molar ratio of (calcium + strontium): sodium carbonate of 1:1.10, and then the pH of the brine is adjusted to 11.5 with sodium hydroxide. After the reaction is completed, the clear liquid is separated from the precipitate by filter pressing, and the pH of the clear liquid is reversely adjusted to 8.0, and then pumped into the evaporation tank, the evaporation temperature is controlled to 75°C, and the vacuum evaporation concentration multiple is 10 times. After the evaporation is completed, the salt slurry is washed with a wash water volume of V (wash water): V (salt slurry) of 1:1, and the washed salt slurry is dried and dehydrated to obtain a low-calcium salt product, and CaCl2 is added to the mother liquor according to the molar ratio of sulfate: calcium chloride of 1:1.1. After the reaction is completed, the precipitate and the clear liquid are separated by filter pressing, and the clear liquid is returned to the raw material pool; finally, the Ca in the low-calcium salt product is 2+ Mg 2+ , SO4 2- and Cl - The content of SO4 in the mother liquor after CaCl2 treatment was tested and the test results are shown in Table 3-1. 2- The content was tested, and the test results are shown in Table 3-2. According to the data results in Table 3-1 and Table 3-2, the total calcium and magnesium ions in industrial dry salt and wet salt are both below 65ppm, and the SO4 in the treated mother liquor is 2- The content is 4.17g / L, close to 4.12g / L in the original brine. Both the salt product and the mother liquor meet the expected indicators.
[0039] Table 3-1 Low calcium salt data detection
[0040]
[0041] Table 3-2 Calcium chloride treatment mother liquor
[0042] Sulfate: Calcium Chloride Molar Ratio <![CDATA[Ca 2+ (g / L)]]> <![CDATA[Mg 2+ (g / L)]]> <![CDATA[SO4 2- (g / L)]]> <![CDATA[Cl - (g / L)]]> 1:1.1 1.51 0 4.17 189
[0043] Example 3
[0044] The gypsum-type brine is decalcified according to the molar ratio of (calcium + strontium): sodium carbonate of 1:1.10, and then the pH of the brine is adjusted to 12.0 with sodium hydroxide. After the reaction is completed, the clear liquid is separated from the precipitate by filter pressing, and the pH of the clear liquid is reversely adjusted to 8.2, and then pumped into the evaporation tank, the evaporation temperature is controlled to 95°C, and the vacuum evaporation concentration multiple is 11 times. After the evaporation is completed, the salt slurry is washed with a wash water volume of V (wash water): V (salt slurry) of 1:1, and the washed salt slurry is dried and dehydrated to obtain a low-calcium salt product, and CaCl2 is added to the mother liquor according to the molar ratio of sulfate: calcium chloride of 1:1. After the reaction is completed, the precipitate and the clear liquid are separated by filter pressing, and the clear liquid is returned to the raw material pool; finally, the Ca in the low-calcium salt product is 2+ Mg 2+ , SO4 2- and Cl - The content of SO4 in the mother liquor after CaCl2 treatment was tested and the test results are shown in Table 4-1. 2- The content was tested, and the test results are shown in Table 4-2. According to the data results in Table 4-1 and Table 4-2, the total calcium and magnesium ions in industrial dry salt and wet salt are both below 61ppm, and the SO4 2- The content is 3.87g / L, slightly lower than the 4.12g / L content in the original brine. 2+ The content of 1.71g / L is slightly higher than the 1.57g / L content in the original brine, and both the salt product and the mother liquor have reached the expected indicators. The main components of the polysilicon wastewater concentrate are shown in the table below:
[0045] Main components of polysilicon wastewater concentrate
[0046] <![CDATA[CaCl2]]> NaCl % % 40 3
[0047] Table 4-1 Low calcium salt data detection
[0048]
[0049] Table 4-2 Calcium chloride treatment mother liquor
[0050] Sulfate: Calcium Chloride Molar Ratio <![CDATA[Ca 2+ (g / L)]]> <![CDATA[Mg 2+ (g / L)]]> <![CDATA[SO4 2- (g / L)]]> <![CDATA[Cl - (g / L)]]> 1:1.14 1.71 0 3.87 189
[0051] Example 4
[0052] The gypsum-type brine is decalcified according to the molar ratio of (calcium + strontium): sodium carbonate of 1:1.10, and then the pH of the brine is adjusted to 11.5 with sodium hydroxide. After the reaction is completed, the clear liquid is separated from the precipitate by filter pressing, and the pH of the clear liquid is reversely adjusted to 8.0, and then pumped into the evaporation tank, the evaporation temperature is controlled to 95°C, and the vacuum evaporation concentration multiple is 10 times. After the evaporation is completed, the salt slurry is washed with a wash water volume of V (wash water): V (salt slurry) of 1:1, and the washed salt slurry is dried and dehydrated to obtain a low-calcium salt product. The mother liquor is added to the polysilicon wastewater concentrate according to the molar ratio of sulfate: calcium chloride of 1:1.14. After the reaction is completed, the precipitate and the clear liquid are separated by filter pressing, and the clear liquid is returned to the raw material pool; finally, the Ca in the low-calcium salt product is 2+ Mg 2+ , SO4 2- and Cl - The content of SO4 in the mother liquor after the treatment of polysilicon wastewater concentrate was tested and the test results are shown in Table 5-1. 2- The content was tested, and the test results are shown in Table 5-2. According to the data results in Table 5-1 and Table 5-2, the total calcium and magnesium ions in industrial dry salt and wet salt are both below 58ppm, and the SO4 2- The content is 3.85g / L, slightly lower than the 4.12g / L content in the original brine. 2+ The content of 1.70g / L is slightly higher than the 1.57g / L content in the original brine, and both the salt product and the mother liquor meet the expected indicators.
[0053] Table 5-1 Low calcium salt data detection
[0054]
[0055] Table 5-2 Mother liquor from polysilicon concentrate treatment
[0056]
[0057]
[0058] Example 5
[0059] The gypsum-type brine is decalcified according to the molar ratio of (calcium + strontium): sodium carbonate of 1:1.10, and then the pH of the brine is adjusted to 11.5 with sodium hydroxide. After the reaction is completed, the clear liquid is separated from the precipitate by filter pressing, and the pH of the clear liquid is reversely adjusted to 8.0, and then pumped into the evaporation tank, the evaporation temperature is controlled to 75°C, and the vacuum evaporation concentration multiple is 10 times. After the evaporation is completed, the salt slurry is washed with a wash water volume of V (wash water): V (salt slurry) of 1:1, and the washed salt slurry is dried and dehydrated to obtain a low-calcium salt product. The mother liquor is added to the polysilicon wastewater concentrate according to the molar ratio of sulfate: calcium chloride of 1:1.1. After the reaction is completed, the precipitate and the clear liquid are separated by filter pressing, and the clear liquid is returned to the raw material pool; finally, the Ca in the low-calcium salt product is2+ Mg 2+ , SO4 2- and Cl - The content of SO4 in the mother liquor after the treatment of polysilicon wastewater concentrate was tested and the test results are shown in Table 6-1. 2- The content was tested, and the test results are shown in Table 6-2. According to the data results in Table 6-1 and Table 6-2, the total calcium and magnesium ions in industrial dry salt and wet salt are both below 66ppm, and the SO4 2- The content is 4.13g / L, close to 4.12g / L in the original brine. Both the salt product and the mother liquor meet the expected indicators.
[0060] Table 6-1 Low calcium salt data detection
[0061]
[0062] Table 6-2 Polysilicon Concentrate Treatment Mother Liquor
[0063] Sulfate: Calcium Chloride Molar Ratio <![CDATA[Ca 2+ (g / L)]]> <![CDATA[Mg 2+ (g / L)]]> <![CDATA[SO4 2- (g / L)]]> <![CDATA[Cl - (g / L)]]> 1:1.1 1.52 0 4.13 189
[0064] Comparative Example 1
[0065] The gypsum-type brine is decalcified according to the molar ratio of (calcium + strontium): sodium carbonate of 1:1.05, and then the pH of the brine is adjusted to 11.5 with sodium hydroxide. After the reaction is completed, the clear liquid is separated from the precipitate by filter pressing, and the pH of the clear liquid is reversely adjusted to 8.0, and then pumped into the evaporation tank, the evaporation temperature is controlled to 75°C, and the vacuum evaporation concentration multiple is 10 times. After the evaporation is completed, the salt slurry is washed with a wash water volume of V (wash water): V (salt slurry) of 1:1, and the washed salt slurry is dried and dehydrated to obtain a low-calcium salt product, and CaCl2 is added to the mother liquor according to the molar ratio of sulfate: calcium chloride of 1:1.0. After the reaction is completed, the precipitate and the clear liquid are separated by filter pressing, and the clear liquid is returned to the raw material pool; finally, the Ca in the low-calcium salt product is 2+ Mg 2+ , SO4 2- and Cl - The content of SO4 in the mother liquor after CaCl2 treatment was tested and the test results are shown in Table 7-1. 2- The content was tested, and the test results are shown in Table 7-2. According to the data results in Table 7-1 and Table 7-2, the total calcium and magnesium ions in industrial dry salt and wet salt are both higher than 120ppm, and the SO4 2- The content is 6.11g / L, which is much higher than the 4.12g / L content in the original brine. 2+ The content of 0.99g / L is slightly lower than the 1.57g / L content in the original brine. Both the salt product and the mother liquor did not meet the expected indicators.
[0066] Table 7-1 Low calcium salt data detection
[0067]
[0068] Table 7-2 Calcium chloride treatment mother liquor
[0069] Sulfate: Calcium Chloride Molar Ratio <![CDATA[Ca 2+ (g / L)]]> <![CDATA[Mg 2+ (g / L)]]> <![CDATA[SO4 2- (g / L)]]> <![CDATA[Cl - (g / L)]]>
[0070] Comparative Example 2
[0071] The gypsum-type brine is decalcified according to the molar ratio of (calcium + strontium): sodium carbonate of 1:1.05, and then the pH of the brine is adjusted to 10.5 with sodium hydroxide. After the reaction is completed, the clear liquid is separated from the precipitate by filter pressing, and the pH of the clear liquid is reversely adjusted to 8.2, and then pumped into the evaporation tank, the evaporation temperature is controlled to 75°C, and the vacuum evaporation concentration multiple is 7.0 times. After the evaporation is completed, the salt slurry is washed with a wash water volume of V (wash water): V (salt slurry) of 1:1, and the washed salt slurry is dried and dehydrated to obtain a low-calcium salt product, and CaCl2 is added to the mother liquor according to the molar ratio of sulfate: calcium chloride of 1:1.05. After the reaction is completed, the precipitate and the clear liquid are separated by filter pressing, and the clear liquid is returned to the raw material pool; finally, the Ca in the low-calcium salt product is 2+ Mg 2+ , SO4 2- and Cl - The content of SO4 in the mother liquor after CaCl2 treatment was tested and the test results are shown in Table 8-1. 2- The content was tested, and the test results are shown in Table 8-2. According to the data results in Table 8-1 and Table 8-2, the total calcium and magnesium ions in industrial dry salt and wet salt are both lower than 120ppm, but the SO4 2- The content is 2.11g / L, which is lower than the 4.12g / L content in the original brine. 2+ The content of 0.73g / L is lower than the content of 1.57g / L in the original brine. The calcium and magnesium ions in the salt product meet the expected standards, but the mother liquor does not meet the expected indicators.
[0072] Table 8-1 Low calcium salt data detection
[0073]
[0074] Table 8-2 Calcium chloride treatment mother liquor
[0075] Sulfate: Calcium Chloride Molar Ratio <![CDATA[Ca 2+ (g / L)]]> <![CDATA[Mg 2+ (g / L)]]> <![CDATA[SO4 2- (g / L)]]> <![CDATA[Cl - (g / L)]]> 1:1.05 0.73 0 2.11 186.7
[0076] Comparative Example 3
[0077] The gypsum-type brine is decalcified according to the molar ratio of (calcium + strontium): sodium carbonate of 1:1.05, and then the pH of the brine is adjusted to 10.5 with sodium hydroxide. After the reaction is completed, the clear liquid is separated from the precipitate by filter pressing, and the pH of the clear liquid is reversely adjusted to 8.2, and then pumped into the evaporation tank, the evaporation temperature is controlled to 75°C, and the vacuum evaporation concentration multiple is 12.0 times. After the evaporation is completed, the salt slurry is washed with a wash water volume of V (wash water): V (salt slurry) of 1:1, and the washed salt slurry is dried and dehydrated to obtain a low-calcium salt product, and CaCl2 is added to the mother liquor according to the molar ratio of sulfate: calcium chloride of 1:1.05. After the reaction is completed, the precipitate is separated from the clear liquid by filter pressing, and the clear liquid is returned to the raw material pool; finally, the Ca in the low-calcium salt product is 2+ Mg 2+ , SO4 2- and Cl - The content of SO4 in the mother liquor after CaCl2 treatment was tested and the test results are shown in Table 9-1. 2- The content was tested, and the test results are shown in Table 9-2. According to the data results in Table 9-1 and Table 9-2, the total calcium and magnesium ions in industrial dry salt and wet salt are both lower than 120ppm, but the SO4 2- The content is 5.23g / L, which is higher than the 4.12g / L content in the original brine. 2+ The content of 2.11g / L is higher than the 1.57g / L content in the original brine. The calcium and magnesium ions in the salt product meet the expected standards, but the mother liquor does not meet the expected indicators.
[0078] Table 9-1 Low calcium salt data detection
[0079]
[0080] Table 9-2 Calcium chloride treatment mother liquor
[0081] Sulfate: Calcium Chloride Molar Ratio <![CDATA[Ca 2+ (g / L)]]> <![CDATA[Mg 2+ (g / L)]]> <![CDATA[SO4 2- (g / L)]]> <![CDATA[Cl - (g / L)]]> 1:1.05 2.11 0 5.23 186.7
[0082] Experiment 1:
[0083] The operation was carried out on the basis of Example 1, the only difference being that the molar ratio of (calcium + strontium) to sodium carbonate was different during the brine pretreatment process, and the parameters of the other steps were the same. The specific results are as follows:
[0084] Table 10 Brine pretreatment
[0085]
[0086] According to the data results in Table 10, six conditions were preliminarily screened out: (calcium + strontium): sodium carbonate molar ratio of 1:1, pH of 12, 1:1.05, pH of 12, 1:1.1, pH of 11.5, 1:1.1, pH of 12, 1:1.15, pH of 11.5, 1:1.15, pH of 12. After comprehensive consideration, considering the investment in equipment and materials, the sodium carbonate molar ratio of 1:1.1 and pH of 11.5 were screened out as the most suitable hardness reduction treatment conditions.
[0087] Experiment 2:
[0088] Based on Example 1, the difference in mother liquor components under different vacuum evaporation concentration multiples and the difference in wet salt components under different concentration multiples were determined, as shown in the following table:
[0089] Table 11 Wet salt composition at different concentration multiples
[0090]
[0091] It can be seen from Table 11 that the salt composition is significantly different at different vacuum evaporation concentration multiples. When the evaporation concentration multiple is ≤11, the salt product produced meets the quality standards. (Note: In order to increase the yield of salt and reduce costs in production, the concentration multiple is generally increased as much as possible while ensuring the quality of salt.)
[0092] Experiment 3:
[0093] The experiment was conducted on the basis of Example 1, the only difference being that the mother liquor was treated with calcium chloride having a mass concentration of 40% (see Table 12-1) or the mother liquor was treated with concentrated polysilicon wastewater (see Table 12-2). The experimental results of treating the mother liquor with different amounts of calcium chloride added were measured, as shown in the following table:
[0094] Table 12-1 Experimental results of treating mother liquor with 40% calcium chloride
[0095] Calcium chloride addition amount <![CDATA[Ca 2+ (g / L)]]> <![CDATA[Mg 2+ (g / L)]]> <![CDATA[SO4 2- (g / L)]]> <![CDATA[Cl - (g / L)]]> 90% 0.73 0 9.34 189.6 95% 0.81 0 7.60 190 100% 0.99 0 6.11 191 105% 1.25 0 5.03 188 110% 1.51 0 4.17 189 114% 1.71 0 3.87 189 118% 1.83 0 3.21 189.5
[0096] According to the data in Table 12-1, as the calcium ion concentration in the solution increases, the sulfate ion gradually decreases. Adding calcium chloride can effectively remove the sulfate ion in the mother liquor. When the amount of calcium chloride added reaches 110% of the theoretical reaction amount, the calcium ion and sulfate ion in the clear liquid after the mother liquor treatment are close to the original water, so 110% is selected as the experimental condition for removing sulfate ion.
[0097] Table 12-2 Experimental results of polysilicon wastewater concentrate
[0098] Wastewater addition amount <![CDATA[Ca 2+ (g / L)]]> <![CDATA[Mg 2+ (g / L)]]> <![CDATA[SO4 2- (g / L)]]> <![CDATA[Cl - (g / L)]]> 90% 0.75 0 9.55 189.9 95% 0.80 0 7.57 190.3 100% 0.95 0 6.02 190.5 105% 1.20 0 5.42 189.4 110% 1.48 0 4.09 189.8 114% 1.77 0 3.83 189.6 118% 1.82 0 3.23 189.2
[0099] According to the data in Table 12-2, the experimental results of the polysilicon wastewater concentrate are basically the same as those of the mother liquor treated with 40% calcium chloride.
[0100] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. A method for producing low-calcium salt from calcium sulfate brine, characterized in that The following steps are involved: Gypsum-type brine is used as raw material, and the raw material is passed into a pretreatment reaction tank. The calcium and magnesium content in the brine is first removed to below 15 mg / L by a two-alkali method, and then the precipitated material is filtered; the clear liquid obtained by filtering is pumped into an evaporation salt making device, vacuum evaporated and concentrated at a certain temperature, and the salt slurry is discharged. The salt slurry is washed with refined brine, and then dehydrated and dried to make a low-calcium salt product; in the low-calcium salt product, the total calcium and magnesium ions are reduced to below 70 ppm; a solution containing calcium chloride is added to the evaporated mother liquor obtained in the vacuum evaporation and concentration step to reduce the sulfate concentration in the mother liquor. After the reaction is completed, the clear liquid is returned to the pretreatment reaction tank, the precipitated material is filtered, and the filtrate is returned to the evaporation mother liquor tank; the two-alkali method The two alkalis are caustic soda and soda ash; the specific steps of removing the total amount of calcium and magnesium in the brine to less than 15 mg / L by the two-alkali method are: first passing sodium carbonate into the gypsum-type brine to remove calcium, then adjusting the pH of the brine with sodium hydroxide, and separating the clear liquid and the precipitate by filter pressing after the reaction is completed; the amount of sodium carbonate added is based on the molar ratio of calcium + strontium to sodium carbonate of 1:1.05-1.15; the pH value of the brine is adjusted to 11.0-12.0 with sodium hydroxide; the temperature of vacuum evaporation concentration is 50°C-110°C, and the vacuum evaporation concentration multiple is 8-11 times; the amount of calcium chloride-containing solution added is based on the molar ratio of sulfate to calcium chloride in the evaporation mother liquor = 1:1.06-1.
14.
2. The method for producing low-calcium salt from calcium sulfate type brine as claimed in claim 1, characterized in that: After vacuum evaporation and concentration, the salt slurry is washed with refined brine, and the salt slurry is washed according to the washing water volume of V washing water: V salt slurry = 1-2:
1.
3. The method for producing low-calcium salt from calcium sulfate type brine as claimed in claim 1, characterized in that: The solution containing calcium chloride is calcium chloride solution, polysilicon wastewater containing calcium chloride or a mixture of the two.
4. The method for producing low-calcium salt from calcium sulfate type brine as claimed in claim 1, characterized in that: The salt slurry is washed with refined brine, and the washing frequency is 1 time.
5. The method for producing low-calcium salt from calcium sulfate type brine as claimed in claim 1, characterized in that: The amount of sodium carbonate added is based on a molar ratio of calcium + strontium to sodium carbonate of 1:1.1; sodium hydroxide is used to adjust the pH value of the brine to 11.
5.
6. A method for producing low-calcium salt from calcium sulfate type brine as described in any one of claims 1 to 5, characterized in that: In the low-calcium salt product, the sulfate ion content is reduced to below 0.30wt%.
Citation Information
Patent Citations
Method for producing refined moisture diffusion industrial salt based on underground recycling of waste liquid
CN103964472A
Method for preparing refined salt low in calcium and magnesium by utilizing underground denitration process
CN103979579A
Preparation method of metal sodium salt
CN104891531A
Technology using calcium and magnesium mud purified by brine to produce magnesium sulfate and calcium sulfate
CN106745115A