Positive electrode sheet of lithium-ion battery and lithium-ion battery
By adopting a multi-layer dressing structure and the outermost lithium replenishing layer in the lithium-ion battery cathode plate, the problems of active lithium loss and gas accumulation in lithium-ion batteries are solved, and the energy density and cycle life of the battery are improved.
Patent Information
- Application Number
- CN202210036637.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-01-13
AI Technical Summary
Lithium-ion batteries will lose active lithium during the first charge and subsequent cycles, resulting in capacity fading. The existing cathode lithium replenishment technology has problems with metal ion dissolution and gas accumulation, which affects battery quality.
The lithium-ion battery cathode plate adopts a multi-layer dressing structure. By setting up multiple layers of dressing layers, the solubility and porosity of the lithium replenishing agent are sequentially increased. Combined with the outermost lithium replenishing layer, the conductivity and gas diffusion efficiency are improved. Prevent dissolution of metal ions and accumulation of gas.
While realizing the lithium replenishment function, it also improves the diffusion rate and uniformity of the electrolyte, increases the energy density of the battery, extends the cycle life of the battery and avoids the problem of black spots on the battery surface.
Smart Images

Figure CN116487520B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of battery preparation, and specifically, the present application relates to a positive electrode sheet of a lithium-ion battery and a lithium-ion battery. Background Art
[0002] In recent years, as my country continues to increase its efforts to promote new energy vehicles, pure electric vehicles with green and environmentally friendly characteristics have become an inevitable trend in the development of the future automobile industry. They will gradually replace traditional fuel buses and become the daily means of transportation for ordinary people. The power source of electric vehicles is lithium-ion batteries. As an important component of electric vehicles, the improvement of various performances of lithium-ion batteries has always been the focus of the industry.
[0003] Generally speaking, lithium-ion batteries will lose active lithium during the initial charging and formation process, and will continue to lose active lithium during subsequent cycles and storage. The loss of active lithium is usually the main reason for the capacity decay of lithium-ion batteries. Therefore, lithium-ion batteries need to be replenished with lithium during the manufacturing process of lithium-ion batteries, including positive electrode replenishment and negative electrode replenishment.
[0004] In the prior art, many side effects occur when lithium is replenished at the positive electrode of a lithium-ion battery, mainly including: first, the main slurry of the positive electrode of the lithium-ion battery generally contains metal ions. While the positive electrode is replenished with lithium, the metal ions will dissolve and migrate to the negative electrode and destroy the passivation layer on the surface of the negative electrode material; second, the lithium replenisher will produce a lot of gas during the lithium replenishment process. The gas cannot be discharged in time and accumulates in the battery electrode and on the surface, resulting in poor battery quality.
[0005] In view of this, a new technical solution needs to be proposed to solve at least one of the above technical problems. Summary of the invention
[0006] One purpose of the embodiments of the present application is to provide a positive electrode plate of a lithium-ion battery and a new technical solution for a lithium-ion battery.
[0007] According to a first aspect of an embodiment of the present application, a positive electrode sheet of a lithium ion battery is provided, and the positive electrode sheet of the lithium ion battery comprises:
[0008] A substrate layer, the substrate layer having a first surface and a second surface disposed opposite to each other; the first surface and / or the second surface are both stacked with at least two dressing layers; each of the dressing layers contains a lithium supplement;
[0009] The solubility of the lithium supplement contained in the dressing layer increases gradually along the direction from close to the substrate layer to far away from the substrate layer.
[0010] Optionally, the first surface and / or the second surface are both provided with a first dressing layer, a second dressing layer, ... an Nth dressing layer, where N is an integer greater than or equal to 2; the first dressing layer is in contact with the substrate layer;
[0011] Wherein, the solubility of the lithium supplement in the first dressing layer is not greater than 0.1 g / 100 g, and the solubility of the lithium supplement in the Nth dressing layer is not less than 1 g / 100 g.
[0012] Optionally, the porosity of the lithium supplement agent contained in the dressing layer increases sequentially along a direction from close to the substrate layer to far away from the substrate layer.
[0013] Optionally, along the direction from close to the substrate layer to far away from the substrate layer, the median particle size of the lithium supplement agent contained in the dressing layer increases successively.
[0014] Optionally, the mass percentage content of the lithium supplement in the dressing layer is 0.05% to 5%.
[0015] Optionally, each dressing layer has a pore structure, and the average pore size of the pore structure in the dressing layer increases successively along the direction from close to the substrate layer to far away from the substrate layer.
[0016] Optionally, along the direction from close to the substrate layer to away from the substrate layer, the dressing layer includes a first dressing layer and a second dressing layer, the first dressing layer contains a first lithium supplement, and the second dressing layer contains a second lithium supplement; the solubility of the first lithium supplement is less than the solubility of the second lithium supplement.
[0017] Optionally, the median particle size of the first lithium supplement is 50 nm to 2 μm, and the mass percentage content of the first lithium supplement in the first dressing layer is 0.05% to 5%;
[0018] The median particle size of the second lithium supplement is 100 nm to 1 μm, and the mass percentage content of the second lithium supplement in the second dressing layer is 0.05% to 5%.
[0019] Optionally, the first lithium supplement includes at least one of lithium carbonate, lithium oxalate, lithium citrate, lithium sulfate and lithium nitrate; and / or the second lithium supplement includes at least one of lithium difluorophosphate, lithium difluorooxalatoborate and lithium bis(fluorosulfonyl)imide.
[0020] Optionally, it is characterized in that a lithium supplement layer is provided on the outermost layer of the dressing layer away from the substrate layer, and the lithium supplement layer contains a lithium supplement agent.
[0021] Optionally, the lithium supplement agent in the lithium supplement layer includes at least one of lithium carbonate, lithium oxalate, lithium citrate, lithium fluoride, lithium phosphate and lithium sulfate.
[0022] Optionally, the median particle size of the lithium supplement agent in the lithium supplement layer is 50 nm to 2 μm.
[0023] Optionally, the first surface and the second surface are both sequentially stacked with a first dressing layer, a second dressing layer and a lithium supplement layer, the first dressing layer contains a first lithium supplement agent, the second dressing layer contains a second lithium supplement agent, and the lithium supplement layer contains a third lithium supplement agent;
[0024] The first lithium supplement has a first solubility in the electrolyte, the second lithium supplement has a second solubility in the electrolyte, and the third lithium supplement has a third solubility in the electrolyte. The first solubility and the third solubility are both smaller than the second solubility.
[0025] Optionally, the mass of the third lithium supplement accounts for 0.05% to 10% of the total mass of the first dressing layer and the second dressing layer.
[0026] Optionally, the first dressing layer has a first pore structure, the second dressing layer has a second pore structure, and the lithium supplement layer has a third pore structure;
[0027] The average pore size of the first pore structure is smaller than the average pore size of the second pore structure, and the average pore size of the second pore structure is smaller than the average pore size of the third pore structure.
[0028] According to a second aspect of an embodiment of the present application, a lithium-ion battery is provided, wherein the lithium-ion battery comprises the positive electrode plate of the lithium-ion battery as described in the first aspect.
[0029] One technical effect of the embodiments of the present application is:
[0030] In the positive electrode plate of the lithium-ion battery provided in the embodiment of the present application, at least two dressing layers are provided on the surface of the substrate layer, the dressing layers contain a lithium supplement, and the solubility of the lithium supplement contained in the dressing layers increases successively from close to the substrate layer to far away from the substrate layer. The positive electrode plate disclosed in the present application can realize the basic lithium supplement function by limiting the relationship of the solubility of the lithium supplement in its multi-layer dressing layers, while improving the diffusion rate and uniformity of the electrolyte in the plate, thereby increasing the energy density of the battery.
[0031] Other features and advantages of the present application will become apparent from the following detailed description of exemplary embodiments of the present application with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the application and, together with the description, serve to explain the principles of the application.
[0033] Figure 1 It is a schematic structural diagram of a positive electrode plate of a lithium-ion battery according to an embodiment of the present application. DETAILED DESCRIPTION
[0034] Various exemplary embodiments of the present application will now be described in detail with reference to the accompanying drawings. It should be noted that unless otherwise specifically stated, the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present application.
[0035] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the present application, its application, or uses.
[0036] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0037] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0038] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0039] An embodiment of the present application provides a positive electrode plate of a lithium-ion battery, wherein the positive electrode plate of the lithium-ion battery includes a substrate layer 1, wherein the substrate layer 1 has a first surface and a second surface arranged opposite to each other; at least two dressing layers are stacked on the first surface and / or the second surface; each of the dressing layers contains a lithium supplement; along the direction from close to the substrate layer 1 to away from the substrate layer 1, the solubility of the lithium supplement contained in the dressing layer increases successively.
[0040] In the positive electrode plate of the lithium-ion battery provided in the embodiment of the present application, in addition to being able to realize the basic lithium supplementation function, it can also be realized: First, the lithium supplementation agent in the dressing layer closer to the substrate layer 1 has a certain solubility in the electrolyte, that is, the lithium supplementation agent can dissociate lithium ions and its anions, and the anions can have a strong binding ability with the metal ions in the positive electrode main slurry, such as divalent Fe ions and trivalent Fe ions. Specifically, the complex formed by the anions and the divalent Fe ions and trivalent Fe ions meets the characteristics of low solubility in the electrolyte or poor conductivity or not easy to be reduced at low potential of the negative electrode, so that the metal ions in the positive electrode main slurry can be prevented from dissolving and migrating to the negative electrode and destroying the passivation layer on the surface of the negative electrode material. Second, the lithium supplementation agent in the dressing layer farther away from the substrate layer 1 has a higher solubility in the electrolyte. When it is dissolved in the electrolyte, a certain pore structure will be left at the position it occupies. The pore structure provides a channel for the flow of gas, which can help to smoothly discharge the gas generated during the lithium supplementation process.
[0041] Furthermore, the first surface and / or the second surface are provided with a first dressing layer, a second dressing layer...an Nth dressing layer, N is an integer greater than or equal to 2, and the first dressing layer is in contact with the substrate layer; wherein the solubility of the lithium supplement in the first dressing layer is not greater than 0.1g / 100g, and the solubility of the lithium supplement in the Nth dressing layer is not less than 1g / 100g.
[0042] Furthermore, a lithium supplement layer 4 is provided on the outermost layer of the dressing layer away from the substrate layer 1 , and the lithium supplement layer 4 contains a lithium supplement agent.
[0043] In this specific example, a lithium replenishing layer 4 is separately provided in the outermost layer, and the lithium replenishing layer 4 only contains a lithium replenishing agent. Firstly, this can avoid introducing too much lithium replenishing agent into the positive electrode main slurry of the dressing layer, thereby avoiding the process problem of poor coating caused by adding too much lithium replenishing agent into the positive electrode main slurry; secondly, since the lithium replenishing agent is mixed with the positive electrode main slurry, the effective conductive agent content per unit volume space in the positive electrode main slurry will be diluted, and the conductivity of the lithium replenishing agent itself is poor, so the charging lithium replenishing effect will be affected to a certain extent. Therefore, by setting a lithium replenishing layer 4 separately in the outermost layer, the content of lithium replenishing agent introduced into the positive electrode main slurry in the dressing layer can be reduced, thereby increasing the effective conductive agent content per unit volume space in the positive electrode main slurry; and generally, the content of conductive agent in the dressing layer is originally low, while the separately set lithium replenishing layer 4 can have a higher conductive agent content, which can improve the conductive effect; in addition, the lithium replenishing layer 4 is in the outermost layer, and it contacts the electrolyte more fully, which is beneficial to improving the lithium replenishing efficiency, and is also beneficial to shortening the diffusion distance of the gas generated during the lithium replenishing process, and accelerating the gas discharge.
[0044] The following takes the setting of two dressing layers and the setting of lithium supplement layer 4 as an example to explain the relevant parameters in detail; Figure 1 As shown, the first surface and the second surface are sequentially stacked with a first dressing layer 2, a second dressing layer 3 and a lithium supplement layer 4, the first dressing layer 2 contains a first lithium supplement agent, the second dressing layer 3 contains a second lithium supplement agent, and the lithium supplement layer 4 contains a third lithium supplement agent; the first lithium supplement agent has a first solubility in the electrolyte, the second lithium supplement agent has a second solubility in the electrolyte, and the third lithium supplement agent has a third solubility in the electrolyte, and the first solubility and the third solubility are both less than the second solubility.
[0045] In one embodiment, further, the first lithium supplement includes at least one of lithium carbonate, lithium oxalate, lithium citrate, lithium sulfate and lithium nitrate.
[0046] In this specific example, the first lithium supplement is selected from one or a combination of two or more of lithium carbonate, lithium oxalate, lithium citrate, lithium sulfate and lithium nitrate; the above lithium supplement is not only a lithium compound that has a certain potential for lithium removal and is not easy to reversibly insert lithium, but also has stable chemical properties in the air. The above lithium supplement has a certain solubility in the electrolyte, that is, it is slightly soluble in the electrolyte, and can dissociate lithium ions and their anions.
[0047] In one embodiment, further, the median particle size of the first lithium supplement agent is 50 nm to 2 μm.
[0048] In this specific example, the first lithium supplement agent is ground to a particle size of 50nm<D50<2μm by ball milling or other processes, and can further be 50nm~500nm. When the median particle size is greater than 500nm, the specific surface area of the first lithium supplement agent is small and the lithium supplement activity is low; and when the median particle size is less than 50nm, the ball milling cost will be greatly increased.
[0049] In one embodiment, further, the mass percentage content of the first lithium supplement in the first dressing layer 2 is 0.05% to 5%.
[0050] In this specific example, the amount of the first lithium supplement agent added is set to 0.05% to 5%, and further optionally 0.1% to 2%, of the total mass of the first dressing layer 2. When the amount of the first lithium supplement agent added is less than 0.05%, the lithium supplement effect is not obvious; and when the amount of the first lithium supplement agent added is higher than 5%, although the amount of lithium supplement is large, the lithium supplement utilization rate is low, and the excessively high content of the first lithium supplement agent and the positive electrode main slurry are easily prone to cause the slurry to be too viscous, agglomerate, and other process problems during the slurry stirring process.
[0051] In one embodiment, further, the second lithium supplement includes at least one of lithium difluorophosphate, lithium difluorooxalatoborate and lithium bis(fluorosulfonyl)imide.
[0052] In this specific example, the second lithium supplement is selected from one or a combination of two or more of lithium difluorophosphate, lithium difluorooxalate borate and lithium bis(fluorosulfonyl)imide; the above lithium supplement is not only a lithium compound with a certain potential for lithium removal and not easy to reversibly insert lithium, but also has stable chemical properties in the air. The above lithium supplement has good solubility in the electrolyte, that is, it is easily soluble in the electrolyte. After the lithium battery is filled and aged, the second lithium supplement is dissolved in the electrolyte, leaving certain pores at the position it occupies; and the second lithium supplement also has a good positive and / or negative electrode film-forming effect, and can form a good protective effect on the positive and / or negative electrode; in addition, since the second lithium supplement is easily soluble in the electrolyte, it can also be used as an electrolyte lithium salt to supplement the lithium salt lost during the lithium supplement process, without the need to use an electrolyte with a higher lithium salt concentration, thereby reducing the problem of wetting and slow liquid absorption of the electrode sheet caused by the high viscosity of the electrolyte.
[0053] In one embodiment, further, the median particle size of the second lithium supplement agent is 100 nm to 1 μm.
[0054] In this specific example, the second lithium supplement is ground to a particle size of 50nm to 1μm by ball milling or other processes. When the median particle size is greater than 1μm, the compactness and energy density of the second dressing layer 3 cannot be well guaranteed; and when the median particle size is less than 50nm, the ball milling cost will be greatly increased, and it is not conducive to the diffusion of the electrolyte.
[0055] In one embodiment, further, the mass percentage content of the second lithium supplement in the second dressing layer 3 is 0.05% to 5%.
[0056] In this specific example, the amount of the second lithium supplement agent added is set to 0.05% to 5% of the total mass of the second dressing layer 3, and can be further set to 0.2% to 2%. When the amount of the second lithium supplement agent added is less than 0.05%, the lithium supplement effect is not obvious; and when the amount of the second lithium supplement agent added is higher than 5%, the lithium supplement amount is large but the lithium supplement utilization rate is low, and the excessively high content of the second lithium supplement agent and the positive electrode main slurry are easily prone to cause the slurry to be too viscous and agglomerate during the slurry stirring process.
[0057] In one embodiment, further, the third lithium supplement includes at least one of lithium carbonate, lithium oxalate, lithium citrate, lithium fluoride, lithium phosphate and lithium sulfate.
[0058] In this specific example, the third lithium supplement is selected from one or a combination of two or more of lithium carbonate, lithium oxalate, lithium citrate, lithium fluoride, lithium phosphate and lithium sulfate; the above lithium supplement is not only a lithium compound with a certain potential for lithium removal and not easy to reversibly insert lithium, but also has stable chemical properties in the air. The above lithium supplement has a certain solubility in the electrolyte, that is, it is slightly soluble in the electrolyte. Since the lithium supplement layer 4 adopts a coating process to form pattern pores, the third lithium supplement is slightly soluble in the electrolyte, which is conducive to retaining the pattern. If the solubility of the third lithium supplement in the electrolyte is large, it will easily make the pattern disappear.
[0059] In one embodiment, further, the median particle size of the third lithium supplement agent is 50 nm to 2 μm.
[0060] In this specific example, the third lithium supplement agent is ground to a particle size of 50nm to 2μm by ball milling or other processes, and further to 50nm to 500nm. When the median particle size is greater than 500nm, the specific surface area of the third lithium supplement agent is small and the lithium supplement activity is low; and when the median particle size is less than 50nm, the ball milling cost will be greatly increased.
[0061] In one embodiment, further, the mass of the third lithium supplement accounts for 0.05% to 10% of the total mass of the first dressing layer 2 and the second dressing layer 3 .
[0062] In this specific example, the amount of the third lithium supplement is set to 0.05% to 10% of the total mass of the first dressing layer 2 and the second dressing layer 3, and can be further set to 0.2% to 5%. When the amount of the third lithium supplement is less than 0.05%, the lithium supplement effect is not obvious; and when the amount of the third lithium supplement is greater than 10%, the lithium supplement amount is large but the lithium supplement utilization rate is low.
[0063] In one embodiment, further, the first dressing layer 2 has a first pore structure, the second dressing layer 3 has a second pore structure, and the lithium supplement layer 4 has a third pore structure; the average pore size of the first pore structure is smaller than the average pore size of the second pore structure, and the average pore size of the second pore structure is smaller than the average pore size of the third pore structure.
[0064] More specifically, the pore size of the first pore structure in the first dressing layer 2 is jointly determined by the particle size and solubility of the first lithium supplement; the pore size of the second pore structure in the second dressing layer 3 is jointly determined by the particle size and solubility of the second lithium supplement; and since the lithium supplement layer 4 adopts a coating process to form pattern pores, the pore size of the third pore structure of the lithium supplement layer 4 is determined by the size of the coated pattern pores. More specifically, the first pore structure is a nanopore with an average pore size of 20 to 50 nm, the second pore structure is a submicron pore with an average pore size of 50 nm to 1 μm, and the third pore structure is a micron pore with an average pore size of 1 μm to 20 μm. The pore structure formed from small to large from the inside to the outside can quickly guide the gas generated during the lithium supplement reaction compared to the single-layer pore structure in the prior art, thereby improving the lithium supplement efficiency while avoiding problems such as surface black spots caused by large accumulation of gas. In addition, when the battery is activated and used subsequently, the pore structure from small to large from the inside to the outside is also conducive to the reflux of the electrolyte, accelerating the reflux speed of the electrolyte, which is beneficial to the long cycle of the battery.
[0065] The present application embodiment provides a method for preparing a positive electrode sheet of a lithium ion battery as described above, which comprises:
[0066] S101, providing a substrate layer 1, wherein the substrate layer 1 has a first surface and a second surface disposed opposite to each other;
[0067] S102, mixing and stirring the positive electrode main slurry, the first lithium supplement agent, the conductive agent, the binder and the solvent to prepare a first slurry;
[0068] S103, mixing and stirring the positive electrode main slurry, the second lithium supplement agent, the conductive agent, the binder and the solvent to prepare the second slurry;
[0069] S104, mixing and stirring a third lithium supplement agent, a conductive agent, a binder and a solvent to prepare a third slurry;
[0070] S105, coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively in sequence, so as to obtain the positive electrode sheet of the lithium ion battery.
[0071] More specifically, the main positive electrode slurry is lithium iron phosphate; the first lithium supplement agent is selected from one or a combination of two or more of lithium carbonate, lithium oxalate, and lithium citrate; the second lithium supplement agent is selected from one or a combination of two or more of lithium difluorophosphate, lithium difluorooxalatoborate, and lithium bis(fluorosulfonyl)imide; the third lithium supplement agent is selected from one or a combination of two or more of lithium carbonate, lithium oxalate, lithium citrate, lithium fluoride, lithium phosphate, and lithium sulfate.
[0072] In one embodiment, further, the coating method of the third slurry includes gravure roller coating or spray coating. Further, the coating shape of the third slurry is a quadrilateral, such as a rectangle, diamond or other quadrilateral pattern, that is, the lithium supplement layer 4 is pore-formed by the coating pattern technology.
[0073] An embodiment of the present application further provides a lithium-ion battery, which includes the positive electrode plate of the lithium-ion battery as described above.
[0074] Embodiment 1:
[0075] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0076] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0077] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0078] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0079] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0080] Embodiment 2:
[0081] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0082] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0083] S103, mixing lithium iron phosphate, lithium difluoroborate oxalate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluoroborate oxalate is 1%; and the median particle size of lithium difluoroborate oxalate is 200 nm;
[0084] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0085] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0086] Embodiment 3:
[0087] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0088] S102, mixing lithium iron phosphate, lithium carbonate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium carbonate is 1%; and the median particle size of the lithium carbonate is 100 nm.
[0089] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0090] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0091] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0092] Embodiment 4:
[0093] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0094] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of the lithium oxalate is 100 nm.
[0095] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0096] S104, mixing and stirring a third lithium replenisher composed of lithium oxalate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium oxalate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium oxalate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0097] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0098] Embodiment 5:
[0099] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0100] S102, mixing lithium iron phosphate, lithium carbonate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium carbonate is 1%; and the median particle size of the lithium carbonate is 100 nm.
[0101] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0102] S104, mixing and stirring a third lithium replenisher composed of lithium oxalate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium oxalate: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium oxalate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0103] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0104] Embodiment 6:
[0105] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0106] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of the lithium oxalate is 100 nm.
[0107] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0108] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 200 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0109] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0110] Embodiment 7:
[0111] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0112] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of the lithium oxalate is 100 nm.
[0113] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0114] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 500 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0115] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0116] Example 8.1:
[0117] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0118] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of the lithium oxalate is 100 nm.
[0119] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0120] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 1 μm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0121] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0122] Example 8.2:
[0123] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0124] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of the lithium oxalate is 100 nm.
[0125] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0126] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 2 μm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0127] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0128] Example 9.1:
[0129] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0130] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of the lithium oxalate is 100 nm.
[0131] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 100 nm;
[0132] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0133] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0134] Example 9.2:
[0135] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0136] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of the lithium oxalate is 100 nm.
[0137] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 500 nm;
[0138] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0139] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0140] Embodiment 10:
[0141] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0142] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of the lithium oxalate is 100 nm.
[0143] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 1 μm;
[0144] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0145] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0146] Example 10.1:
[0147] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0148] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 50 nm.
[0149] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 500 nm;
[0150] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 500 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0151] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0152] Example 10.2:
[0153] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0154] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 2 μm.
[0155] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 500 nm;
[0156] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 500 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0157] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0158] Embodiment 11:
[0159] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0160] S102, mixing and stirring lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 500 nm.
[0161] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0162] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0163] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0164] Embodiment 12:
[0165] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0166] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; wherein the median particle size of the lithium oxalate is 1 μm.
[0167] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; wherein the median particle size of lithium difluorophosphate is 200 nm;
[0168] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0169] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0170] Example 12.1:
[0171] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0172] S102, mixing and stirring lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 500 nm.
[0173] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 800 nm;
[0174] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0175] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0176] Embodiment 13:
[0177] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0178] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0179] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; wherein the median particle size of lithium difluorophosphate is 200 nm;
[0180] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0181] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0182] Embodiment 14:
[0183] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0184] S102, mixing and stirring lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 3%; and the median particle size of lithium oxalate is 100 nm.
[0185] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; wherein the median particle size of lithium difluorophosphate is 200 nm;
[0186] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0187] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0188] Embodiment 15:
[0189] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0190] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 0.07%; and the median particle size of lithium oxalate is 100 nm.
[0191] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; wherein the median particle size of lithium difluorophosphate is 200 nm;
[0192] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0193] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0194] Embodiment 16:
[0195] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0196] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0197] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0198] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0199] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0200] Embodiment 17:
[0201] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0202] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0203] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 3%; and the median particle size of lithium difluorophosphate is 200 nm;
[0204] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0205] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0206] Embodiment 18:
[0207] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0208] S102, mixing and stirring lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to obtain a first slurry; wherein the mass percentage content of lithium oxalate is 1%; wherein the median particle size of the lithium oxalate is 100 nm.
[0209] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0210] S104, coating the first slurry and the second slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125g / m 2 The coating surface density of the second slurry is 125g / m 2 , and then rolling the first slurry and the second slurry to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0211] Embodiment 19:
[0212] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0213] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 0.05%; and the median particle size of lithium oxalate is 100 nm.
[0214] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0215] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 500 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0216] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0217] Embodiment 20:
[0218] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0219] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 5%; and the median particle size of lithium oxalate is 100 nm.
[0220] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0221] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 200 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0222] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0223] Embodiment 21:
[0224] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0225] S102, mixing and stirring lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 0.1%; and the median particle size of lithium oxalate is 100 nm.
[0226] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0227] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 500 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0228] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0229] Embodiment 22:
[0230] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0231] S102, mixing and stirring lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 2%; and the median particle size of lithium oxalate is 100 nm.
[0232] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0233] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 500 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0234] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0235] Embodiment 23:
[0236] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0237] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0238] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 0.05%; and the median particle size of lithium difluorophosphate is 200 nm;
[0239] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0240] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0241] Embodiment 24:
[0242] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0243] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0244] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 5%; and the median particle size of lithium difluorophosphate is 200 nm;
[0245] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0246] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0247] Embodiment 25:
[0248] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0249] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0250] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 0.1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0251] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0252] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0253] Embodiment 26:
[0254] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0255] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0256] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 2%; and the median particle size of lithium difluorophosphate is 200 nm;
[0257] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0258] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0259] Embodiment 27:
[0260] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0261] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0262] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0263] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 0.05% of the total mass of the first slurry and the second slurry;
[0264] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0265] Embodiment 28:
[0266] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0267] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0268] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0269] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 10% of the total mass of the first slurry and the second slurry;
[0270] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0271] Embodiment 29:
[0272] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0273] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0274] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0275] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 0.2% of the total mass of the first slurry and the second slurry;
[0276] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0277] Embodiment 30:
[0278] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0279] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0280] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0281] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 5% of the total mass of the first slurry and the second slurry;
[0282] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0283] Embodiment 31:
[0284] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0285] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 200 nm.
[0286] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0287] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0288] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0289] Embodiment 32:
[0290] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0291] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 200 nm.
[0292] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0293] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 200 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0294] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0295] Embodiment 33:
[0296] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0297] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 20 nm.
[0298] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0299] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0300] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0301] Embodiment 34:
[0302] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0303] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 3 μm.
[0304] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0305] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0306] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0307] Embodiment 35:
[0308] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0309] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 0.02%; and the median particle size of lithium oxalate is 100 nm.
[0310] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0311] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0312] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0313] Embodiment 36:
[0314] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0315] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 10%; and the median particle size of lithium oxalate is 100 nm.
[0316] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0317] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0318] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0319] Embodiment 37:
[0320] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0321] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0322] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 30 nm;
[0323] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0324] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0325] Embodiment 38:
[0326] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0327] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0328] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 2 μm;
[0329] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0330] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0331] Embodiment 39:
[0332] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0333] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0334] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 0.01%; and the median particle size of lithium difluorophosphate is 200 nm;
[0335] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0336] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0337] Embodiment 40:
[0338] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0339] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0340] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 10%; and the median particle size of lithium difluorophosphate is 200 nm;
[0341] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0342] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0343] Embodiment 41:
[0344] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0345] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0346] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0347] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 3 μm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0348] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0349] Embodiment 42:
[0350] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0351] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0352] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0353] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 20 nm; and the mass of the third lithium replenisher is 1% of the total mass of the first slurry and the second slurry;
[0354] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0355] Embodiment 43:
[0356] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0357] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0358] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0359] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 0.02% of the total mass of the first slurry and the second slurry;
[0360] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0361] Embodiment 44:
[0362] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0363] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein the mass percentage content of lithium oxalate is 1%; and the median particle size of lithium oxalate is 100 nm.
[0364] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein the mass percentage content of lithium difluorophosphate is 1%; and the median particle size of lithium difluorophosphate is 200 nm;
[0365] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, in terms of mass percentage, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm; and the mass of the third lithium replenisher is 20% of the total mass of the first slurry and the second slurry;
[0366] S105, sequentially coating the first slurry, the second slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0367] A portion of the positive electrode sheets prepared in the above embodiment was tested for liquid absorption time and porosity; another portion of the positive electrode sheets and the double-sided surface density of 245 g / m 2 The negative electrode sheet of graphite material is assembled into a soft-pack battery, and the soft-pack battery is baked, injected, infiltrated, formed, aged, exhausted, and divided into finished batteries. The formation process parameters are charging at 0.05C for 2 hours at a temperature of 35-45°C, and then charging to 4.0V at a constant current and constant voltage of 0.2C, and then charging at a constant voltage until the current drops to 0.05C, and charging stops; then charging to 4.55V at a constant current of 0.05C, and then charging at a constant voltage until the current drops to 0.005C, and charging stops; and the first discharge capacity is tested. The finished battery is cycled at 60°C and 1C rate (3.8V→2.0V range), and the number of 80% SOH cycles is obtained by testing. The specific experimental results are shown in the subsequent Table 1.
[0368] Comparative Example 1:
[0369] The positive electrode of the lithium-ion battery is made of lithium iron phosphate coated aluminum foil; wherein the coating surface density is 125g / m 2 , roller compacted to a compaction density of 2.55 g / ml.
[0370] A portion of the positive electrode sheets prepared in the above comparative example 1 was tested for liquid absorption time and porosity; another portion of the positive electrode sheets and the double-sided surface density of 245 g / m 2 The negative electrode sheet of graphite material is assembled into a soft-pack battery, and the soft-pack battery is baked, injected, infiltrated, formed, aged, exhausted, and divided into finished batteries. The formation process parameters are charging at 0.05C for 2 hours at a temperature of 35-45°C, then charging to 3.8V at 0.2C constant current and constant voltage, and then charging at constant voltage until the current drops to 0.003C, and charging stops; and the first discharge capacity is tested. The finished battery is cycled at 60°C and 1C rate (3.8V→2.0V range), and the number of 80% SOH cycles is obtained by testing. The specific experimental results are shown in the subsequent Table 1.
[0371] Comparative Example 2:
[0372] The positive electrode of the lithium-ion battery is made of lithium iron phosphate coated aluminum foil; wherein the coating surface density is 125g / m 2 , roller compacted to a compaction density of 2.55 g / ml.
[0373] Comparative Example 3:
[0374] Lithium iron phosphate, lithium oxalate, lithium difluorophosphate, lithium carbonate, lithium fluoride, conductive agent, binder and solvent are mixed and stirred to prepare slurry and coated on aluminum foil to prepare positive electrode sheet; wherein the coating surface density is 125g / m 2 , roller compacted to a compaction density of 2.55 g / ml.
[0375] Comparative Example 4:
[0376] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0377] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein, according to the mass ratio, lithium iron phosphate: lithium oxalate: conductive agent: binder: solvent = 95:1:1.5:2.5:70; wherein the median particle size of lithium oxalate is 100 nm.
[0378] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein, according to the mass ratio, lithium iron phosphate: lithium difluorophosphate: conductive agent: binder: solvent = 95.5:0.5:1.5:2.5:70; wherein the median particle size of lithium difluorophosphate is 200 nm;
[0379] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, according to the mass ratio, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm;
[0380] S105, sequentially coating the second slurry, the first slurry and the third slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0381] Comparative Example 5:
[0382] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0383] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein, according to the mass ratio, lithium iron phosphate: lithium oxalate: conductive agent: binder: solvent = 95:1:1.5:2.5:70; wherein the median particle size of lithium oxalate is 100 nm.
[0384] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein, according to the mass ratio, lithium iron phosphate: lithium difluorophosphate: conductive agent: binder: solvent = 95.5:0.5:1.5:2.5:70; wherein the median particle size of lithium difluorophosphate is 200 nm;
[0385] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, according to the mass ratio, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm;
[0386] S105, sequentially coating the third slurry, the first slurry and the second slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0387] Comparative Example 6:
[0388] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0389] S102, mixing lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to prepare a first slurry; wherein, according to the mass ratio, lithium iron phosphate: lithium oxalate: conductive agent: binder: solvent = 95:1:1.5:2.5:70; wherein the median particle size of lithium oxalate is 100 nm.
[0390] S103, mixing lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder and a solvent to prepare a second slurry; wherein, according to the mass ratio, lithium iron phosphate: lithium difluorophosphate: conductive agent: binder: solvent = 95.5:0.5:1.5:2.5:70; wherein the median particle size of lithium difluorophosphate is 200 nm;
[0391] S104, mixing and stirring a third lithium replenisher composed of lithium carbonate and lithium fluoride, a conductive agent, a binder and a solvent to prepare a third slurry; wherein, according to the mass ratio, lithium carbonate: lithium fluoride: conductive agent: binder: solvent = 75:10:10:5:70; wherein, the median particle size of the third lithium replenisher composed of lithium carbonate and lithium fluoride is 50 nm;
[0392] S105, sequentially coating the first slurry, the third slurry and the second slurry on the first surface and the second surface respectively; wherein the coating surface density of the first slurry is 125 g / m 2 The coating surface density of the second slurry is 125g / m 2 The coating surface density of the third slurry is 5g / m 2 Then, the first slurry, the second slurry and the third slurry are rolled to a compaction density of 2.55 g / ml; thus, the positive electrode sheet of the lithium ion battery is obtained.
[0393] Comparative Example 7:
[0394] S101, providing an aluminum foil, wherein the aluminum foil has a first surface and a second surface disposed opposite to each other;
[0395] S102, mixing and stirring lithium iron phosphate, lithium oxalate, a conductive agent, a binder, and a solvent to obtain a first slurry; mixing and stirring lithium iron phosphate, lithium difluorophosphate, a conductive agent, a binder, and a solvent to obtain a second slurry; mixing the first slurry and the second slurry to obtain a slurry mixture;
[0396] S104, mixing and stirring a third lithium supplement agent composed of lithium carbonate and lithium fluoride, a conductive agent, a binder, and a solvent to prepare a third slurry;
[0397] S105, coating the slurry mixture and the third slurry on the first surface and the second surface respectively in sequence; that is, obtaining the positive electrode sheet of the lithium ion battery.
[0398] A portion of the positive electrode sheets prepared in Comparative Examples 2 to 7 was tested for liquid absorption time and porosity; another portion of the positive electrode sheets and the double-sided surface density of 245 g / m 2The negative electrode sheet of graphite material is assembled into a soft-pack battery, and the soft-pack battery is baked, injected, infiltrated, formed, aged, exhausted, and divided into finished batteries. The formation process parameters are charging at 0.05C for 2 hours at a temperature of 35-45°C, and then charging to 4.0V at a constant current and constant voltage of 0.2C, and then charging at a constant voltage until the current drops to 0.05C, and charging stops; then charging to 4.55V at a constant current of 0.05C, and then charging at a constant voltage until the current drops to 0.005C, and charging stops; and the first discharge capacity is tested. The finished battery is cycled at 60°C and 1C rate (3.8V→2.0V range), and the number of 80% SOH cycles is obtained by testing. The specific experimental results are shown in the subsequent Table 1.
[0399] Performance test results:
[0400] 1) Porosity and liquid absorption time test of positive electrode
[0401] The porosity of the positive electrode was tested by mercury intrusion method; the liquid absorption time of the positive electrode was measured by contact angle test equipment to observe the time from initial contact to complete absorption (contact angle 0 degrees) of the dropped electrolyte droplets.
[0402] 2) Battery charge and discharge performance test
[0403] After aging, exhausting and vacuum sealing, the soft-pack batteries obtained in each embodiment and comparative example were discharged to 2.0V at a constant current of 0.6A at room temperature, and the total charging capacity and discharging capacity of the battery for the first charge were recorded. The charge and discharge efficiency (%) was calculated as charging capacity / discharging capacity×100%.
[0404] 3) Battery high temperature cycle test
[0405] The battery was charged to 3.8V at 1C constant current at 60°C, and then discharged to 2.0V at 1C constant current; the charge and discharge cycle was repeated 500 times; the discharge capacity of the 500th cycle was recorded, and the capacity retention rate after the cycle (%) was calculated as follows: discharge capacity of 500 cycles / first discharge capacity × 100%. The cycle was continued until the capacity decayed to 80% of the initial capacity, and the total number of cycles was recorded.
[0406] The test results are shown in Table 1.
[0407] Table 1:
[0408]
[0409]
[0410]
[0411] As shown in Table 1, first, when the porosity is the same or similar, the shorter the liquid absorption time, the better the performance of the positive electrode sheet, because the shorter the liquid absorption time means the faster the diffusion rate of the gas and liquid phase. More specifically, as shown in Table 1, for example, the porosity of the positive electrode sheet prepared in Example 1 is 28.8% and the liquid absorption time is 123S; the porosity of the positive electrode sheet prepared in Comparative Example 1 is 28.3% and the liquid absorption time is 173S; the porosity of the former is only 1.7% higher than that of the latter, while the liquid absorption time of the former is 28.9% shorter than that of the latter, indicating that the performance of the positive electrode sheet prepared in Example 1 is superior to that of the positive electrode sheet prepared in Comparative Example 1.
[0412] For example, the porosity of the positive electrode sheet prepared in Example 1 is 28.8%, and the liquid absorption time is 123S; the porosity of the positive electrode sheet prepared in Comparative Example 3 is 28.0%, and the liquid absorption time is 226S; the porosity of the former is only 2.8% greater than that of the latter, while the liquid absorption time of the former is 45.6% shorter than that of the latter, indicating that the performance of the positive electrode sheet prepared in Example 1 is superior to that of the positive electrode sheet prepared in Comparative Example 1.
[0413] In Example 18, since the outermost lithium replenishing layer 4 is not provided, the charge and discharge performance and high temperature cycle performance of the corresponding battery are not as good as those in Example 1. In Example 8.1, the particle size of the third lithium replenisher is larger, and the charge and discharge performance and high temperature cycle performance of the corresponding battery are not as good as those in Example 1. In Example 8.1, the particle size of the first lithium replenisher is larger, and the charge and discharge performance and high temperature cycle performance of the corresponding battery are not as good as those in Example 1. In Example 31, the particle sizes of the first lithium replenisher and the second lithium replenisher are equal, and in Example 32, the particle sizes of the first lithium replenisher, the second lithium replenisher and the third lithium replenisher are all equal; while in Example 7, the particle sizes of the first lithium replenisher, the second lithium replenisher and the third lithium replenisher increase successively, and the initial efficiency and capacity retention rate of the batteries corresponding to Examples 31 and 32 are not as good as those in Example 7.
[0414] In Examples 33 to 44, the particle size or content of the lithium supplement agent exceeds the preferred range, and the corresponding initial efficiency and capacity retention rate of the battery are not as good as those in Example 1.
[0415] Since no lithium supplement agent was provided in Comparative Examples 1 and 2, the initial efficiency and capacity retention rate of the corresponding batteries were not as good as those in Example 1. The lithium supplement agent in Comparative Example 3 was not layered, and the initial efficiency and capacity retention rate of the corresponding batteries were not as good as those in Example 1. The first lithium supplement agent, the second lithium supplement agent, and the third lithium supplement agent in Comparative Examples 4, 5, 6, and 7 were not layered in sequence, and the initial efficiency and capacity retention rate of the corresponding batteries were not as good as those in Example 1.
[0416] As shown in Table 1, for example, the first charge capacity of the positive electrode plate prepared in Example 1 is 2346 mAh, the first discharge capacity is 2043 mAh, and the first efficiency is 87.1%; the first charge capacity of the positive electrode plate prepared in Comparative Example 1 is 2132 mAh, the first discharge capacity is 1878 mAh, and the first efficiency is 88.1%; although the first efficiency of the former is 1.1% lower than the first efficiency of the latter, the first charge capacity and the first discharge capacity of the former are 9.1% and 8% larger than the first charge capacity and the first discharge capacity of the latter, respectively; therefore, the comprehensive performance of the positive electrode plate prepared in Example 1 is superior to the comprehensive performance of the positive electrode plate prepared in Comparative Example 1.
[0417] For example, the first charging capacity of the positive electrode plate prepared in Example 20 is 1923mAh, the first discharge capacity is 1702mAh, and the first efficiency is 88.5%; the first charging capacity of the positive electrode plate prepared in Comparative Example 8 is 1889mAh, the first discharge capacity is 1655mAh, and the first efficiency is 87.6%; the first charging capacity, first discharge capacity and first efficiency of the former are greater than the first charging capacity, first discharge capacity and first efficiency of the latter, so the comprehensive performance of the positive electrode plate prepared in Example 20 is superior to the comprehensive performance of the positive electrode plate prepared in Comparative Example 8.
[0418] For example, the first charging capacity of the positive electrode plate prepared in Example 21 is 1947mAh, the first discharge capacity is 1729mAh, and the first efficiency is 88.8%; the first charging capacity of the positive electrode plate prepared in Comparative Example 9 is 1925mAh, the first discharge capacity is 1694mAh, and the first efficiency is 88.0%; the first charging capacity, first discharge capacity and first efficiency of the former are greater than the first charging capacity, first discharge capacity and first efficiency of the latter, so the comprehensive performance of the positive electrode plate prepared in Example 21 is superior to the comprehensive performance of the positive electrode plate prepared in Comparative Example 9.
[0419] For example, the first charging capacity of the positive electrode plate prepared in Example 22 is 1494mAh, the first discharge capacity is 1356mAh, and the first efficiency is 90.8%; the first charging capacity of the positive electrode plate prepared in Comparative Example 10 is 1489mAh, the first discharge capacity is 1348mAh, and the first efficiency is 90.5%; the first charging capacity, first discharge capacity and first efficiency of the former are greater than the first charging capacity, first discharge capacity and first efficiency of the latter, so the comprehensive performance of the positive electrode plate prepared in Example 22 is superior to the comprehensive performance of the positive electrode plate prepared in Comparative Example 10.
[0420] In addition, it can be seen from Table 1 that although the positive electrode sheet prepared in Comparative Example 10 has the shortest liquid absorption time, its first charge capacity and first discharge capacity are also relatively small, so its overall performance is not superior.
[0421] As shown in Table 1, for example, the positive electrode sheet prepared in Example 1 has an initial discharge capacity of 2043 mAh, a discharge capacity of 1984 mAh after 500 cycles, a capacity retention rate of 97.1%, and a cycle number of cycles to 80% of the initial capacity of more than 1500; the positive electrode sheet prepared in Comparative Example 1 has an initial discharge capacity of 1878 mAh, a discharge capacity of 1733 mAh after 500 cycles, a capacity retention rate of 92.3%, and a cycle number of cycles to 80% of the initial capacity of 1200; the initial discharge capacity, discharge capacity after 500 cycles, capacity retention rate, and cycle number of cycles to 80% of the initial capacity of the former are all greater than those of the latter, so the comprehensive performance of the positive electrode sheet prepared in Example 1 is superior to the comprehensive performance of the positive electrode sheet prepared in Comparative Example 1.
[0422] For example, the positive electrode sheet prepared in Example 1 has an initial discharge capacity of 2043 mAh, a discharge capacity of 1984 mAh after 500 cycles, a capacity retention rate of 97.1%, and a cycle number of cycles to 80% of the initial capacity of more than 1500; the positive electrode sheet prepared in Comparative Example 2 has an initial discharge capacity of 1910 mAh, a discharge capacity of 1748 mAh after 500 cycles, a capacity retention rate of 91.5%, and a cycle number of cycles to 80% of the initial capacity of 1000; the initial discharge capacity, discharge capacity after 500 cycles, capacity retention rate, and cycle number of cycles to 80% of the initial capacity of the former are all greater than those of the latter, so the comprehensive performance of the positive electrode sheet prepared in Example 1 is superior to the comprehensive performance of the positive electrode sheet prepared in Comparative Example 2.
[0423] For example, the positive electrode sheet prepared in Example 19 has an initial discharge capacity of 2018 mAh, a discharge capacity of 1965 mAh after 500 cycles, a capacity retention rate of 97.4%, and a cycle number of cycles to 80% of the initial capacity of more than 1500; the positive electrode sheet prepared in Comparative Example 7 has an initial discharge capacity of 1994 mAh, a discharge capacity of 1930 mAh after 500 cycles, a capacity retention rate of 96.8%, and a cycle number of cycles to 80% of the initial capacity of more than 1500; although the number of cycles to 80% of the initial capacity of the former is equivalent to that of the latter, the initial discharge capacity, the discharge capacity after 500 cycles and the capacity retention rate of the former are all greater than those of the latter. Therefore, the comprehensive performance of the positive electrode sheet prepared in Example 19 is superior to the comprehensive performance of the positive electrode sheet prepared in Comparative Example 7.
[0424] For example, the positive electrode sheet prepared in Example 21 has an initial discharge capacity of 1729 mAh, a discharge capacity of 1686 mAh after 500 cycles, a capacity retention rate of 97.5%, and a number of cycles to 80% of the initial capacity of more than 1500; the positive electrode sheet prepared in Comparative Example 9 has an initial discharge capacity of 1694 mAh, a discharge capacity of 1635 mAh after 500 cycles, a capacity retention rate of 96.5%, and a number of cycles to 80% of the initial capacity of more than 1500; although the number of cycles to 80% of the initial capacity of the former is equivalent to that of the latter, the initial discharge capacity, discharge capacity after 500 cycles and capacity retention rate of the former are all greater than those of the latter. Therefore, the comprehensive performance of the positive electrode sheet prepared in Example 21 is superior to the comprehensive performance of the positive electrode sheet prepared in Comparative Example 9.
[0425] Although some specific embodiments of the present application have been described in detail by way of example, it should be understood by those skilled in the art that the above examples are only for illustration, not for limiting the scope of the present application. It should be understood by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present application. The scope of the present application is defined by the appended claims.
Claims
1. A positive electrode sheet for a lithium-ion battery, It is characterized in that The positive electrode plate of the lithium-ion battery comprises: A substrate layer (1), the substrate layer (1) having a first surface and a second surface disposed opposite to each other; the first surface and / or the second surface are both laminated with at least two dressing layers; each of the dressing layers contains a lithium supplement; The solubility of the lithium supplement contained in the dressing layer far from the substrate layer (1) in the electrolyte is greater than the solubility of the lithium supplement contained in the dressing layer close to the substrate layer (1) in the electrolyte; The substrate layer (1) is aluminum foil; the dressing layer is composed of a positive electrode main slurry, a lithium supplement agent, a conductive agent, a binder and a solvent.
2. The positive electrode sheet of the lithium ion battery according to claim 1, It is characterized in that The first surface and / or the second surface are both provided with a first dressing layer, a second dressing layer, ... an Nth dressing layer, where N is an integer greater than or equal to 2; the first dressing layer is in contact with the substrate layer (1); Wherein, the solubility of the lithium supplement in the first dressing layer is not greater than 0.1 g / 100 g, and the solubility of the lithium supplement in the Nth dressing layer is not less than 1 g / 100 g.
3. The positive electrode sheet of the lithium ion battery according to claim 1, It is characterized in that The porosity of the lithium supplement contained in the dressing layer far from the substrate layer (1) is greater than the porosity of the lithium supplement contained in the dressing layer close to the substrate layer (1).
4. The positive electrode sheet of the lithium ion battery according to claim 1, It is characterized in that The median particle size of the lithium supplement contained in the dressing layer far from the substrate layer (1) is larger than the median particle size of the lithium supplement contained in the dressing layer close to the substrate layer (1).
5. The positive electrode sheet of the lithium ion battery according to claim 1, It is characterized in that The mass percentage content of the lithium supplement in the dressing layer is 0.05% to 5%.
6. The positive electrode sheet of the lithium ion battery according to claim 1, It is characterized in that Each dressing layer has a pore structure, and the average pore size of the pore structure in the dressing layer far from the substrate layer (1) is larger than the average pore size of the pore structure in the dressing layer close to the substrate layer (1).
7. The positive electrode sheet of the lithium ion battery according to claim 1, It is characterized in that Along the direction from close to the substrate layer (1) to far away from the substrate layer (1), the dressing layer comprises a first dressing layer (2) and a second dressing layer (3), the first dressing layer (2) comprises a first lithium supplement, and the second dressing layer (3) comprises a second lithium supplement; the solubility of the first lithium supplement in the electrolyte is less than the solubility of the second lithium supplement in the electrolyte.
8. The positive electrode sheet of the lithium ion battery according to claim 7, It is characterized in that The median particle size of the first lithium supplement is 50 nm to 2 μm, and the mass percentage content of the first lithium supplement in the first dressing layer (2) is 0.05% to 5%; The median particle size of the second lithium supplement is 100 nm to 1 μm, and the mass percentage content of the second lithium supplement in the second dressing layer (3) is 0.05% to 5%.
9. The positive electrode sheet of the lithium ion battery according to claim 7, It is characterized in that The first lithium supplement includes at least one of lithium carbonate, lithium oxalate, lithium citrate, lithium sulfate and lithium nitrate; and / or the second lithium supplement includes at least one of lithium difluorophosphate, lithium difluorooxalatoborate and lithium bis(fluorosulfonyl)imide.
10. The positive electrode sheet of a lithium ion battery according to any one of claims 1 to 9, It is characterized in that The outermost layer of the dressing layer away from the substrate layer (1) is provided with a lithium supplement layer (4), and the lithium supplement layer (4) contains a lithium supplement agent.
11. The positive electrode sheet of the lithium ion battery according to claim 10, It is characterized in that The lithium supplementing agent in the lithium supplementing layer (4) includes at least one of lithium carbonate, lithium oxalate, lithium citrate, lithium fluoride, lithium phosphate and lithium sulfate.
12. The positive electrode sheet of the lithium ion battery according to claim 11, It is characterized in that The median particle size of the lithium replenishing agent in the lithium replenishing layer (4) is 50 nm to 2 μm.
13. The positive electrode sheet of the lithium ion battery according to claim 1, It is characterized in that The first surface and the second surface are both sequentially stacked with a first dressing layer (2), a second dressing layer (3) and a lithium supplement layer (4), the first dressing layer (2) comprising a first lithium supplement agent, the second dressing layer (3) comprising a second lithium supplement agent, and the lithium supplement layer (4) comprising a third lithium supplement agent, a conductive agent, a binder and a solvent; The first lithium supplement has a first solubility in the electrolyte, the second lithium supplement has a second solubility in the electrolyte, and the third lithium supplement has a third solubility in the electrolyte. The first solubility and the third solubility are both smaller than the second solubility.
14. The positive electrode sheet of the lithium ion battery according to claim 13, It is characterized in that The mass of the third lithium supplement accounts for 0.05% to 10% of the total mass of the first dressing layer (2) and the second dressing layer (3).
15. The positive electrode sheet of the lithium ion battery according to claim 13, It is characterized in that The first dressing layer (2) has a first pore structure, the second dressing layer (3) has a second pore structure, and the lithium supplement layer (4) has a third pore structure; The average pore size of the first pore structure is smaller than the average pore size of the second pore structure, and the average pore size of the second pore structure is smaller than the average pore size of the third pore structure.
16. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the positive electrode sheet of the lithium-ion battery according to any one of claims 1 to 15.
Citation Information
Patent Citations
A lithium-supplemented electrode of a negative electrode of a lithium ion battery and a preparation method thereo
CN109103419A