A strontium titanate thin film suitable for degrading dyeing and printing wastewater, its preparation method and application

By preparing strontium titanate thin films on porous SiC ceramic substrates, the problem of low reusability of strontium titanate powder catalysts was solved, the photocatalytic degradation efficiency of dyeing and printing wastewater was improved, and the stability and high efficiency of the films were achieved.

CN116550353BActive Publication Date: 2026-11-10WUHAN INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310639857.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2026-11-10
Estimated Expiration
2043-05-29

AI Technical Summary

Technical Problem

Existing strontium titanate powder catalysts have low reusability and are difficult to maintain high catalytic activity when degrading dyeing and printing wastewater.

Method used

By uniformly loading strontium titanate thin films onto porous SiC ceramic substrates and preparing them using a sol-gel method, including low-temperature complexation, spin-coating, and calcination steps, a stable strontium titanate thin film is formed, ensuring that the pores between the film and the substrate are not blocked, thus enhancing photocatalytic activity.

Benefits of technology

This technology enables the repeated use of strontium titanate membranes, maintains the filtration performance of the substrate, enhances the contact area between wastewater and the membrane, significantly improves photocatalytic degradation efficiency, and is green, efficient, and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004261260850000011
    Figure HDA0004261260850000011
  • Figure HDA0004261260850000012
    Figure HDA0004261260850000012
  • Figure HDA0004261260850000013
    Figure HDA0004261260850000013
Patent Text Reader

Abstract

This invention discloses a strontium titanate thin film suitable for degrading dyeing and printing wastewater, its preparation method, and its application. The strontium titanate thin film is uniformly loaded onto a porous SiC ceramic substrate. It is prepared by low-temperature complexation of isopropyl titanate and an organic complexing agent, followed by the formation of a SrTiO3 sol with strontium nitrate solution and PEG 2000. After aging, the sol is spin-coated onto the porous SiC ceramic substrate, and finally dried and calcined. The organic complexing agent is diethanolamine or ethanolamine, and the molar ratio of isopropyl titanate to the organic complexing agent is 1:2-6. The low-temperature complexation temperature is 0-4℃. This strontium titanate thin film retains the pollutant filtration properties of the substrate while enhancing the photocatalytic activity for pollutant degradation. It also allows for repeated use of the film, making it green, efficient, and environmentally friendly, with broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of functional materials, specifically relating to a strontium titanate thin film suitable for degrading dyeing and printing wastewater, its preparation method, and its application. Background Technology

[0002] Textile dyeing and printing wastewater is one of the major sources of industrial wastewater. Due to the variety of dyes, the wastewater has a complex composition, high organic content, and poor biodegradability, making its treatment one of the most challenging aspects of industrial wastewater treatment today. Color removal is key to treating dyeing and printing wastewater, and photocatalytic technology can effectively degrade organic pollutants.

[0003] Strontium titanate (SrTiO3) is a common catalyst with a typical perovskite structure, characterized by low toxicity, good thermal stability, and high catalytic activity. In recent years, numerous researchers have studied and reported on the catalytic activity of SrTiO3, such as photocatalytic water splitting for hydrogen production and photocatalytic degradation of organic pollutants. However, the reusability of SrTiO3 powder catalysts is low, and primary use is not conducive to recovery. Therefore, improving the catalytic activity of SrTiO3 while simultaneously achieving its reusability is a pressing issue. Summary of the Invention

[0004] In view of this, to overcome the above-mentioned shortcomings, the purpose of this invention is to provide a strontium titanate thin film suitable for degrading dyeing and printing wastewater, its preparation method, and its application. This strontium titanate thin film retains the pollutant filtration properties of the substrate while enhancing the photocatalytic activity for pollutant degradation, and enables repeated use of the film, making it green, efficient, and environmentally friendly.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows:

[0006] A strontium titanate thin film suitable for degrading dyeing and printing wastewater is provided. The strontium titanate thin film is uniformly loaded on a porous SiC ceramic substrate. It is prepared by low-temperature complexation of isopropyl titanate and an organic complexing agent, followed by the formation of SrTiO3 sol with strontium nitrate solution and PEG 2000. After aging, the sol is deposited on the porous SiC ceramic substrate by spin coating and finally dried and calcined. The organic complexing agent is diethanolamine or ethanolamine, the molar ratio of isopropyl titanate to organic complexing agent is 1:2-6, and the low-temperature complexation temperature is 0-4℃.

[0007] A method for preparing strontium titanate thin films suitable for degrading dyeing and printing wastewater is provided, comprising the following steps:

[0008] 1) After mixing isopropyl titanate and organic complexing agent evenly, add anhydrous ethanol and continue mixing evenly. Let stand at 0-4℃ to fully complex and obtain solution A; wherein the organic complexing agent is diethanolamine or ethanolamine, and the molar ratio of isopropyl titanate to organic complexing agent is 1:2-6.

[0009] 2) Mix strontium nitrate with deionized water until homogeneous to obtain solution B;

[0010] 3) Under the condition of vigorous stirring of solution A obtained in step 1), solution B obtained in step 2) is added dropwise to solution A, stirred evenly, and then nonionic surfactant PEG 2000 is added, and stirring is continued until SrTiO3 sol is formed.

[0011] 4) After the SrTiO3 sol obtained in step 3) is allowed to stand for aging, it is coated on a porous SiC ceramic substrate by spin coating, dried and calcined to obtain a strontium titanate film suitable for degrading dyeing and printing wastewater.

[0012] In the above scheme, the complexation time in step 1) is 0.5 to 1 hour.

[0013] In the above scheme, in step 1), the molar ratio of isopropyl titanate to anhydrous ethanol is 1:1 to 3.

[0014] In the above scheme, in step 2), the molar ratio of strontium nitrate to water is 1:1 to 5.

[0015] In the above scheme, the molar ratio of isopropyl titanate in step 1) to strontium nitrate in step 2) is 1:1.

[0016] In the above scheme, the molar ratio of strontium nitrate in step 2) to PEG2000 in step 3) is 1:0.5~1.

[0017] In the above scheme, in step 4), the aging temperature is 20-30℃ and the aging time is 0.5-1h.

[0018] In the above scheme, in step 4), the drying temperature is 60-80℃ and the drying time is 0.5-1h.

[0019] In the above scheme, in step 4), the calcination temperature is 600-900℃ and the holding time is 3-5h.

[0020] This invention provides an application of the aforementioned strontium titanate thin film in the degradation of dyeing and printing wastewater.

[0021] The beneficial effects of this invention are:

[0022] 1. This invention provides a strontium titanate membrane suitable for degrading dyeing and printing wastewater. The porous strontium titanate membrane is uniformly distributed on a porous SiC substrate without collapse or blockage of the substrate pores. It retains the substrate's ability to filter pollutants while enhancing the photocatalytic activity for pollutant degradation. It also enables repeated use of the membrane, making it green, efficient, and environmentally friendly.

[0023] 2. This invention provides a method for preparing strontium titanate thin films suitable for degrading dyeing and printing wastewater. First, a strontium titanate precursor sol is obtained using a sol-gel method, then spin-coated onto a porous SiC ceramic substrate and finally calcined to obtain the final film. Specifically, isopropyl titanate and an excess organic complexing agent are complexed at a low temperature of 0-4℃. The excess organic complexing agent effectively inhibits the hydrolysis of the complex salt, resulting in stable complex salt properties, reduced intermolecular thermal motion, and a uniform and stable gel with strong intermolecular interactions. The porous strontium titanate thin film obtained by spin-coating onto the porous SiC substrate is uniform, crack-free, and does not collapse, preserving the pores of the matrix. This method is simple to operate, easy to control, has good process repeatability and film quality, and has broad industrial application prospects.

[0024] 3. The porous strontium titanate film prepared by the method of the present invention grows firmly on the porous SiC substrate without clogging the substrate pores, retaining the filtration performance of the porous SiC substrate. In the process of wastewater filtration, it greatly increases the contact area between wastewater and the film, thereby increasing its photocatalytic performance. At the same time, it also enables repeated use of the film, making it green, efficient and environmentally friendly. Attached Figure Description

[0025] Figure 1 This is a scanning electron microscope image of the thin film in Embodiment 1 of the present invention.

[0026] Figure 2 This is a scanning electron microscope image of the cross-section of the thin film in Embodiment 1 of the present invention.

[0027] Figure 3 The results are from photocatalytic application experiments using the sample obtained in Example 1, the sample in Comparative Example 2, and the SiC substrate. Detailed Implementation

[0028] To better understand the present invention, the following embodiments further illustrate the content of the present invention, but the content of the present invention is not limited to the following embodiments.

[0029] Example 1:

[0030] A method for preparing strontium titanate thin films suitable for degrading dyeing and printing wastewater is provided, comprising the following steps:

[0031] 1) Stir 12.5 mmol of isopropyl titanate and 25 mmol of diethanolamine in a 4°C water bath, then add 30 mmol of anhydrous ethanol and continue stirring. Let stand for 30 min to fully complex and form an isopropyl titanate ethanol solution, i.e., solution A.

[0032] 2) Prepare a strontium nitrate aqueous solution (solution B) by mixing 12.5 mmol of strontium nitrate with 50 mmol of deionized water;

[0033] 3) Under vigorous stirring, slowly add solution B to solution A. After stirring, add 10 mmol of nonionic surfactant PEG 2000 and continue stirring until SrTiO3 sol is formed.

[0034] 4) The obtained SrTiO3 sol was left to stand at 20℃ for 30 minutes to reach a suitable viscosity before coating.

[0035] 5) A strontium titanate film was obtained by spin coating on a clean SiC ceramic substrate. The substrate coated with SrTiO3 sol was dried at 60°C for 1 hour and then kept at 600°C for 3 hours in a muffle furnace.

[0036] Figure 1 The image shown is a scanning electron microscope (SEM) image of the thin film in this embodiment. The image shows that a complete strontium titanate thin film was formed and the film has many tiny pores.

[0037] Figure 2 The image shows a scanning electron microscope (SEM) image of the cross-section of the thin film in this embodiment. The image shows that there is a complete strontium titanate thin film on the surface, and the underlying SiC substrate is still porous. During the formation of the strontium titanate thin film, the film did not collapse and block the pores.

[0038] Example 2:

[0039] A method for preparing strontium titanate thin films suitable for degrading dyeing and printing wastewater is provided, comprising the following steps:

[0040] 1) Stir 12.5 mmol of isopropyl titanate and 25 mmol of diethanolamine in a 4°C water bath, then add 30 mmol of anhydrous ethanol and continue stirring. Let stand for 30 min to fully complex and form an isopropyl titanate ethanol solution, i.e., solution A.

[0041] 2) Prepare a strontium nitrate aqueous solution (solution B) by mixing 12.5 mmol of strontium nitrate with 50 mmol of deionized water;

[0042] 3) Under vigorous stirring, slowly add solution B to solution A. After stirring, add 10 mmol of nonionic surfactant PEG 2000 and continue stirring until SrTiO3 sol is formed.

[0043] 4) The obtained SrTiO3 sol was left to stand at 20℃ for 30 minutes to reach a suitable viscosity before coating.

[0044] 5) A strontium titanate thin film was obtained by spin coating on a clean SiC ceramic substrate. The substrate coated with SrTiO3 sol was dried at 60°C for 1 hour and then kept at 700°C for 3 hours in a muffle furnace.

[0045] Example 3:

[0046] A method for preparing strontium titanate thin films suitable for degrading dyeing and printing wastewater is provided, comprising the following steps:

[0047] 1) Stir 12.5 mmol of isopropyl titanate and 25 mmol of diethanolamine in a 4°C water bath, then add 30 mmol of anhydrous ethanol and continue stirring. Let stand for 30 min to fully complex and form an isopropyl titanate ethanol solution, i.e., solution A.

[0048] 2) Prepare a strontium nitrate aqueous solution (solution B) by mixing 12.5 mmol of strontium nitrate with 50 mmol of deionized water;

[0049] 3) Under vigorous stirring, slowly add solution B to solution A. After stirring, add 10 mmol of nonionic surfactant PEG 2000 and continue stirring until SrTiO3 sol is formed.

[0050] 4) The obtained SrTiO3 sol was left to stand at 20℃ for 30 minutes to reach a suitable viscosity before coating.

[0051] 5) A strontium titanate thin film was obtained by spin coating on a clean SiC ceramic substrate. The substrate coated with SrTiO3 sol was dried at 60°C for 1 hour and then kept at 800°C for 3 hours in a muffle furnace.

[0052] Example 4:

[0053] A method for preparing strontium titanate thin films suitable for degrading dyeing and printing wastewater is provided, comprising the following steps:

[0054] 1) Stir 12.5 mmol of isopropyl titanate and 25 mmol of diethanolamine in a 4°C water bath, then add 30 mmol of anhydrous ethanol and continue stirring. Let stand for 30 min to fully complex and form an isopropyl titanate ethanol solution, i.e., solution A.

[0055] 2) Prepare a strontium nitrate aqueous solution (solution B) by mixing 12.5 mmol of strontium nitrate with 50 mmol of deionized water;

[0056] 3) Under vigorous stirring, slowly add solution B to solution A. After stirring, add 10 mmol of nonionic surfactant PEG 2000 and continue stirring until SrTiO3 sol is formed.

[0057] 4) The obtained SrTiO3 sol was left to stand at 20℃ for 30 minutes to reach a suitable viscosity before coating.

[0058] 5) A strontium titanate film was obtained by spin coating on a clean SiC ceramic substrate. The substrate coated with SrTiO3 sol was dried at 60°C for 1 hour and then kept at 900°C for 3 hours in a muffle furnace.

[0059] Comparative Example 1:

[0060] 1) Stir 12.5 mmol of isopropyl titanate and 25 mmol of diethanolamine in a 10°C water bath, then add 30 mmol of anhydrous ethanol and continue stirring. Let stand for 30 min to fully complex and form an isopropyl titanate ethanol solution, i.e., solution A.

[0061] 2) Prepare a strontium nitrate aqueous solution (solution B) by mixing 12.5 mmol of strontium nitrate with 50 mmol of deionized water;

[0062] 3) Under vigorous stirring, slowly add solution B to solution A. After stirring, add 10 mmol of nonionic surfactant PEG 2000 and continue stirring until SrTiO3 sol is formed.

[0063] 4) The obtained SrTiO3 sol was left to stand at 20℃ for 30 minutes to reach a suitable viscosity before coating.

[0064] 5) A strontium titanate film was deposited on a clean SiC ceramic substrate by spin coating. The substrate coated with SrTiO3 sol was dried at 60°C for 1 hour and then kept at 900°C for 3 hours in a muffle furnace. No complete strontium titanate film was obtained.

[0065] Comparative Example 2:

[0066] 1) Stir 12.5 mmol of isopropyl titanate and 25 mmol of diethanolamine in a 4°C water bath, then add 30 mmol of anhydrous ethanol and continue stirring. Let stand for 30 min to fully complex and form an isopropyl titanate ethanol solution, i.e., solution A.

[0067] 2) Prepare a strontium nitrate aqueous solution (solution B) by mixing 12.5 mmol of strontium nitrate with 50 mmol of deionized water;

[0068] 3) Under vigorous stirring, slowly add solution B to solution A. After stirring, add 10 mmol of nonionic surfactant PEG 2000 and continue stirring until SrTiO3 sol is formed.

[0069] 4) The obtained SrTiO3 sol was left to stand at 20℃ for 30 minutes to reach a suitable viscosity before coating.

[0070] 5) A strontium titanate film was obtained by spin coating on a clean quartz glass substrate. The substrate coated with SrTiO3 sol was dried at 60°C for 1 hour and then kept at 600°C for 3 hours in a muffle furnace.

[0071] The results of photocatalytic application experiments were conducted on the sample obtained in Example 1, the sample in Comparative Example 2, and the SiC substrate, as shown below. Figure 3 As shown in the figure, the degradation performance of the SiC substrate was not significant throughout the process, with a degradation rate of 25.3%. In Comparative Example 2, the film was deposited on a dense quartz glass substrate, and in the photocatalytic degradation experiment, wastewater could not pass through the substrate, with a degradation rate of 82.3%. In Example 1, the film was deposited on a porous SiC substrate. In the photocatalytic degradation experiment, due to the porosity of the substrate, water could fully contact the film during the process of passing through the substrate, increasing the contact area and greatly enhancing its degradation performance, with a degradation rate of 95.7%, which is significantly improved compared to Comparative Example 2.

[0072] All the raw materials listed in this invention can achieve this invention, and the upper and lower limits and ranges of each raw material can also achieve this invention; examples are not listed one by one here. The upper and lower limits and ranges of the process parameters (such as temperature, time, etc.) of this invention can also achieve this invention; examples are not listed one by one here.

Claims

1. A strontium titanate thin film suitable for degrading dyeing and printing wastewater, characterized in that, The strontium titanate film is uniformly loaded on a porous SiC ceramic substrate. It is prepared by low-temperature complexation of isopropyl titanate and an organic complexing agent, followed by the formation of SrTiO3 sol with strontium nitrate solution and PEG 2000. After aging for 0.5-1 h, the film is deposited on the porous SiC ceramic substrate by spin coating, and finally dried and calcined. The organic complexing agent is diethanolamine or ethanolamine, the molar ratio of isopropyl titanate to organic complexing agent is 1:2-6, and the low-temperature complexation temperature is 0-4℃.

2. A method for preparing a strontium titanate thin film according to claim 1, characterized in that, Includes the following steps: 1) After mixing isopropyl titanate and organic complexing agent evenly, add anhydrous ethanol and continue mixing evenly. Let stand at 0~4℃ to fully complex and obtain solution A; wherein the organic complexing agent is diethanolamine or ethanolamine, and the molar ratio of isopropyl titanate to organic complexing agent is 1:2-6. 2) Mix strontium nitrate with deionized water until homogeneous to obtain solution B; 3) Under the condition of vigorous stirring of solution A obtained in step 1), solution B obtained in step 2) is added dropwise to solution A, stirred evenly, and then nonionic surfactant PEG 2000 is added, and stirring is continued until SrTiO3 sol is formed. 4) After the SrTiO3 sol obtained in step 3) is left to stand for 0.5 to 1 hour, it is coated on a porous SiC ceramic substrate by spin coating, dried and calcined to obtain a strontium titanate film suitable for degrading dyeing and printing wastewater.

3. The preparation method according to claim 2, characterized in that, In step 1), the complexation time is 0.5~1h.

4. The preparation method according to claim 2, characterized in that, In step 1), the molar ratio of isopropyl titanate to anhydrous ethanol is 1:1~3; in step 2), the molar ratio of strontium nitrate to water is 1:1~5.

5. The preparation method according to claim 2, characterized in that, The molar ratio of isopropyl titanate in step 1) to strontium nitrate in step 2) is 1:

1.

6. The preparation method according to claim 2, characterized in that, The molar ratio of strontium nitrate in step 2) to PEG2000 in step 3) is 1:0.5~1.

7. The preparation method according to claim 2, characterized in that, In step 4), the aging temperature is 20~30℃.

8. The preparation method according to claim 2, characterized in that, In step 4), the drying temperature is 60~80℃ and the drying time is 0.5~1h.

9. The preparation method according to claim 2, characterized in that, In step 4), the calcination temperature is 600~900℃ and the holding time is 3~5h.

10. The application of the strontium titanate film according to claim 1 in the degradation of dyeing and printing wastewater.

Citation Information

Patent Citations

  • Method for preparing strontium titanate film having spherical grain accumulated porous structure

    CN102390935A

  • Preparation method of loaded modified TiO2 film porous ceramic particles and photocatalysis sewage treatment device

    CN106732497A